ME201n · B.Tech Mechanical · End Term

Engineering Materials & Metallurgy

Master notes, solved PYQs and a 12-hour plan, aimed at 30 out of 40

Paper40 marks · 3 hours · answer any 5 of 6 questions · 8 marks each
SplitEach question is 2 parts: 6+2, 5+3 or 4+4
Syllabus6 units, per the DTU scheme (42 contact hours)
SourcesCallister, Materials Science and Engineering (10th ed.); DTU End Sem Nov 2024 (ME201n); Mid Sem Mar 2024
How to use: start with “Read this first” and the PYQ topic map, follow the 12-hour plan, and practise every diagram marked in the units by hand. Sections are tagged High Medium Low by how likely they are to be asked.
Read this first

How to score 30 out of 40

You answer 5 questions out of 6. You can skip one whole question, so prepare five question types thoroughly rather than six halfway.

The paper pattern

The Nov 2024 end-term (ME201n) had six 8-mark questions, each with an (a) and a (b) part. Every question mixed a long theory or diagram answer with a short derivation or numerical. Each question roughly maps to one syllabus area:

QNov 2024 (what was asked)Unit
1(a) Fe–C diagram, all phases, reactions (6) · (b) Derive Gibbs’ phase rule (2)3
2(a) Griffith theory, derive critical stress (6) · (b) Numerical: surface energy from KIc (2)4
3(a) Three powder-production methods + making cemented carbide tools (5) · (b) Annealing vs normalizing, microstructure (3)6, 3
4(a) Three stages of creep + mechanisms (4) · (b) TTT diagram of eutectoid steel, labelled (4)4, 3
5(a) Miller indices procedure, cubic and HCP, with examples (5) · (b) Numerical: vacancies in Cu at 200 °C (3)1
6(a) Reinforcements in polymer-matrix composites (6) · (b) Duralumin and brass: composition, properties, uses (2)5/6, 2
Strategy

PYQ topic map

✓ = asked in that paper. Topics marked High below should not be skipped.

TopicMid 2024End 2024PriorityUnit
Iron–carbon diagram + invariant reactions✓✓High3
TTT diagram, heat treatment (annealing, normalizing, hardening, tempering)✓High3
Gibbs’ phase rule, lever rule✓High3
Griffith theory, fracture toughness numericals✓High4
Creep curve and mechanisms✓High4
APF, a–r relations, planar density✓High1
Interplanar spacing + Bragg’s law✓High1
Miller indices (cubic and HCP)✓High1
Imperfections, edge vs screw dislocation✓High1
Vacancy concentration numerical✓Medium1
Crystal systems: axial relations✓Medium1
Powder production, cemented carbides✓Medium6
Composites: reinforcements, rule of mixtures✓Medium5, 6
Non-ferrous alloys (duralumin, brass)✓Medium2
Fatigue, DBTT, ductile vs brittle fractureMedium4
Case hardening, precipitation hardeningMedium3
Corrosion, galvanic cell, protectionMedium2
Recovery, recrystallization, cold/hot workingMedium1
Alloy, tool and stainless steelsLow2

Not covered in either 2024 paper but on the syllabus: corrosion, fatigue, case hardening, precipitation hardening, recovery and recrystallization. Since they haven't come up recently, expect at least one of them to appear.

12-hour study plan

TimeWhat to doOutput
Hour 0–0:30Read this section, both solved PYQ papers (end of this PDF) and the formula sheet once, quickly. Don’t memorise yet.Know the target
Hour 0:30–3:00Unit 3. Fe–C diagram (draw it 3 times from memory), invariant reactions, lever-rule numericals, Gibbs’ phase rule derivation, TTT diagram, annealing, normalizing, hardening, tempering, case hardening.Q1 + half of Q3/Q4 secured
Hour 3:00–5:00Unit 1. Unit cells, a–r relations, APF, density, planar density, Miller indices (cubic and HCP), d-spacing and Bragg’s law, defects, dislocations, slip vs twinning. Solve every worked numerical yourself.Q5 secured
Hour 5:00–5:20Break. Walk, eat, no phone.
Hour 5:20–7:20Unit 4. Stress–strain and yield point, ductile vs brittle fracture, Griffith derivation (write it twice), KIc numericals, DBTT, fatigue (S–N curve), creep curve + mechanisms + creep-resistant materials.Q2 + creep secured
Hour 7:20–9:00Units 5 + 6. Composite classification tree, rule of mixtures, critical fibre length, fibres (glass, carbon, Kevlar) and matrices, coupling agents. Powder metallurgy steps, powder production, sintering, cemented carbides, advantages.Q6 / PM secured
Hour 9:00–10:15Unit 2. Plain carbon steels, effect of alloying elements (table), stainless and tool steels, non-ferrous alloy table (duralumin, brasses, bronzes), corrosion types, galvanic cell, rusting reactions, protection methods.Backup question
Hour 10:15–11:15Mock: write the Nov 2024 paper in 60 minutes without notes (attempt 5 questions). Check against the solutions.Find gaps
Hour 11:15–12:00Formula sheet, the must-draw diagrams list and the “Likely exam questions” boxes of each unit. Sleep if possible.Final revision

Contents

Unit 1Structure of metals: crystal structures, Miller indices, defects, dislocations, slip and twinning, cold/hot working, recovery and recrystallizationp. 5
Unit 2Materials: plain carbon and alloy steels, tool and stainless steels, non-ferrous alloys; corrosionp. 24
Unit 3Solidification, phase diagrams, iron–carbon diagram, TTT, heat treatment, case hardening, precipitation hardeningp. 38
Unit 4Yield and elastic modulus, fracture, Griffith theory, fracture toughness, DBTT, fatigue; creepp. 58
Unit 5Composite materials: classification, characteristics, rule of mixtures, applicationsp. 73
Unit 6Powder metallurgy; fibre-reinforced composites: fibres, matrices, coupling agents, fillersp. 80
PYQsEnd Sem Nov 2024 (ME201n) and Mid Sem Mar 2024, fully solvedp. 90
RevisionFormula sheet, key numbers, must-draw diagrams, answer-writing checklistp. 100
Unit 1 · ~7 contact hrs

Structure of Metals

Most asked: APF and a–R relations, planar/linear density, Miller indices (cubic + HCP), Bragg's law numericals, number of vacancies, edge vs screw dislocation, recovery–recrystallization–grain growth.
How this unit is examined

Usually 1–2 full questions (8 marks each, split 4+4, 5+3 or 6+2). There's almost always one numerical: planar density, Bragg/d-spacing, vacancies or density. Learn the six worked numericals in this unit. Between them they cover nearly every numerical type the paper uses.

1. Basic terms High

Definitions

Seven crystal systems and 14 Bravais lattices Asked: End Sem 2024

Every crystal belongs to one of 7 systems, set by the axial relationships (a, b, c) and inter-axial angles (α between b and c, β between a and c, γ between a and b). Adding body-, face- and base-centring gives 14 Bravais lattices.

Crystal systemAxial relationshipInter-axial anglesBravais lattices (no.)Example
Cubica = b = cα = β = γ = 90°P, I (BCC), F (FCC) — 3Fe, Cu, NaCl
Tetragonala = b ≠ cα = β = γ = 90°P, I — 2β-Sn, TiO₂
Orthorhombica ≠ b ≠ cα = β = γ = 90°P, I, F, C — 4α-S, Ga
Hexagonala = b ≠ cα = β = 90°, γ = 120°P — 1Zn, Mg, Ti
Rhombohedral (trigonal)a = b = cα = β = γ ≠ 90°P — 1Bi, calcite
Monoclinica ≠ b ≠ cα = γ = 90° ≠ βP, C — 2gypsum
Triclinica ≠ b ≠ cα ≠ β ≠ γ ≠ 90°P — 1K₂Cr₂O₇

P = primitive (simple), I = body-centred, F = face-centred, C = base-centred. Total 3+2+4+1+1+2+1 = 14. Memory hook for most→least symmetric: Cubic, Hexagonal, Tetragonal, Rhombohedral, Orthorhombic, Monoclinic, Triclinic.

2. Metallic crystal structures: SC, BCC, FCC, HCP High

Simple cubic (SC)BCCFCC
Reduced-sphere unit cells. Corner atoms are dark; body-centre (BCC) and face-centre (FCC) atoms are in accent colour. Hidden edges are dashed.

Relationship between lattice parameter a and atomic radius R Asked: End Sem 2024

SC: a = 2RSCface diag: a√2 = 4RFCC (cube face)body diag: a√3 = 4RBCC (section a × a√2)
Atoms touch along the cube edge (SC), the face diagonal (FCC) or the body diagonal (BCC). Always draw this figure before writing the relation.
a–R relations
SC: atoms touch along edge → a = 2R
BCC: body diagonal √3 a = 4R → a = 4R/√3
FCC: face diagonal √2 a = 4R → a = 2√2 R
HCP: a = 2R, ideal c/a = 1.633

Atoms per unit cell

Count each atom by the share of it that lies inside the cell: corner = 1/8, face = 1/2, edge = 1/4, body = 1.

APF derivations (write these fully for 4–5 marks)

APF of SC

n = 1, a = 2R, Vc = 8R³

APF = (1 × 4/3 πR³)/8R³ = π/6 = 0.52

APF of BCC

n = 2, a = 4R/√3 → Vc = 64R³/(3√3)

APF = (2 × 4/3 πR³)/(64R³/3√3) = √3π/8 = 0.68

APF of FCC

n = 4, a = 2√2R → Vc = 16√2 R³

APF = (4 × 4/3 πR³)/(16√2R³) = π/(3√2) = 0.74

APF of HCP

n = 6, a = 2R, c = 1.633a. Base area = (3√3/2)a² = 6√3R²; Vc = base × c = 6√3R² × 3.266R = 33.94R³.

APF = (6 × 4.189R³)/33.94R³ = 0.74

PropertySCBCCFCCHCP
Atoms / cell1246
a vs Ra = 2Ra = 4R/√3a = 2√2Ra = 2R, c = 1.633a
Coordination no.681212
APF0.520.680.740.74
Close-packed planes—none truly ({110} densest){111}(0001) basal
Stacking——ABCABC…ABAB…
Slip systems—12 (48 possible)123
Ductility—moderate; ductile–brittle transitionvery ductile, even at low Tlimited (brittle-ish)
ExamplesPoα-Fe, Cr, Mo, W, VCu, Al, Ni, Ag, Au, γ-Fe, PbZn, Mg, Ti, Cd, Co
caHCP: A B A B …ABAFCC: A B C A B C …ABC
HCP unit cell: 12 corner atoms, 2 basal face centres and 3 atoms in the mid-plane (accent). Right: stacking of close-packed layers. ABAB… gives HCP; ABCABC… gives FCC. Both have CN 12 and APF 0.74.

Density computation

Theoretical density
ρ = n A / (Vc NA)

n = atoms per cell, A = atomic weight (g/mol), Vc = a³ in cm³, NA = 6.022 × 10²³ atoms/mol.

Worked numerical 1: density of Cu and Fe

Cu (FCC), R = 0.128 nm, A = 63.5 g/mol. a = 2√2(0.128) = 0.3620 nm = 3.620 × 10⁻⁸ cm, so Vc = 4.745 × 10⁻²³ cm³.

ρ = (4 × 63.5)/(4.745 × 10⁻²³ × 6.022 × 10²³) = 254/28.58 = 8.89 g/cm³ (measured 8.94).

α-Fe (BCC), R = 0.124 nm, A = 55.85. a = 4(0.124)/√3 = 0.2864 nm, so Vc = 2.348 × 10⁻²³ cm³.

ρ = (2 × 55.85)/(2.348 × 10⁻²³ × 6.022 × 10²³) = 7.90 g/cm³ (measured 7.87).

Reverse form: given ρ, A and the structure, find R. Solve for Vc = nA/(ρNA), then a = Vc1/3, then R from the a–R relation.

3. Miller indices: directions and planes High

Procedure for a crystallographic direction [uvw] (cubic)

  1. Draw a vector through the origin, or note the coordinates of its head and tail in units of a, b, c.
  2. Subtract: head − tail.
  3. Multiply or divide by a common factor to get the smallest integers.
  4. Enclose in square brackets without commas: [uvw]. A negative index is written with a bar, e.g. [1̄10].
  5. Family of equivalent directions: ⟨uvw⟩, e.g. ⟨100⟩ = [100], [010], [001], [1̄00]…

Procedure for a crystallographic plane (hkl) (cubic)

  1. If the plane passes through the origin, shift the origin to a neighbouring corner (or draw a parallel plane).
  2. Write the intercepts on the x, y, z axes in units of a, b, c. A plane parallel to an axis has intercept ∞.
  3. Take the reciprocals (1/∞ = 0).
  4. Clear fractions to the smallest integers. Do not reduce further if the indices came from intercepts.
  5. Write in round brackets: (hkl). Family of planes: {hkl}, e.g. {111}.
Must remember

In cubic crystals only, the direction [hkl] is perpendicular to the plane (hkl). Parallel planes have the same (or negative) indices.

xyz(100)(110)(111)(0 1̄ 2)O′
Common planes in a cubic cell. In the 4th cube the plane would pass through the origin, so O′ is taken at (0,1,0). Intercepts are then ∞, −1, ½, reciprocals 0, −1, 2, giving (0 1̄ 2).
xyz[100][110][111][001][2̄ 2 1]tail (1,0,½)head (0,1,1)
Left: low-index directions from the origin. Right: head − tail = (0,1,1) − (1,0,½) = (−1, 1, ½). Multiplying by 2 gives [2̄ 2 1].
Worked numerical 2: Miller indices

(a) Plane with intercepts x = ½, y = 1, z = ∞ → reciprocals 2, 1, 0 → (210).

(b) Plane with intercepts x = 1, y = −1, z = ½ → reciprocals 1, −1, 2 → (1 1̄ 2).

(c) Plane with intercepts 2a, 3b, ∞ → reciprocals ½, ⅓, 0 → ×6 → (320).

(d) Direction from tail (½, 0, 1) to head (0, 1, 0): head − tail = (−½, 1, −1) → ×2 → [1̄ 2 2̄].

Miller–Bravais indices for HCP (4-index) Asked: End Sem 2024

HCP uses four axes: a₁, a₂, a₃ in the basal plane at 120° to each other, and z (c-axis) perpendicular to them. This makes equivalent planes and directions look equivalent in their indices, e.g. all prism planes are of the form {10 1̄ 0}.

Worked numerical 3: HCP conversions

(a) Convert [010] to 4-index: U = 0, V = 1, W = 0. u = (0 − 1)/3 = −⅓; v = (2 − 0)/3 = ⅔; t = −(−⅓ + ⅔) = −⅓; w = 0. Multiply by 3 → [1̄ 2 1̄ 0].

(b) Convert [111]: u = (2−1)/3 = ⅓; v = (2−1)/3 = ⅓; t = −⅔; w = 1. ×3 → [1 1 2̄ 3].

(c) Plane with intercepts a₁ = 1, a₂ = −1, a₃ = ∞, z = 1: reciprocals 1, −1, 0, 1 → (1 1̄ 0 1). Check: i = −(1 + (−1)) = 0 ✓.

Linear and planar density Asked: End Sem 2024

Formulas
LD = (no. of atoms whose centres lie on the direction vector) / (length of vector)
PD = (no. of atoms centred on the plane, within the cell) / (area of plane within the cell)

Count only atoms whose centres lie on the line or plane. A plane corner atom contributes ¼ (rectangle) or ⅙ (60° triangle corner), an edge atom ½, and an atom at the centre of the plane 1.

length = a√2 = 4Rheighta = 2√2RFCC (110) plane — 2 atomsside = 4R; 3×⅙ + 3×½ = 2 atomsFCC (111) plane — densest
FCC (110): a rectangle 4R × 2√2R holding 4 × ¼ + 2 × ½ = 2 atoms. FCC (111): a triangle of side 4R holding 2 atoms.
Worked numerical 4: planar density in terms of R (and for Cu, Fe)

FCC (100): square of side a = 2√2R, area 8R². Atoms = 4 × ¼ + 1 = 2. PD = 2/8R² = 1/(4R²) = 0.25/R²

FCC (110): rectangle a√2 × a = 4R × 2√2R, area 8√2R². Atoms = 4 × ¼ + 2 × ½ = 2. PD = 2/(8√2R²) = 1/(4√2R²) = 0.177/R²

FCC (111): equilateral triangle of side 4R, area = (√3/4)(4R)² = 4√3R². Atoms = 3 × ⅙ + 3 × ½ = 2. PD = 2/(4√3R²) = 1/(2√3R²) = 0.289/R². This is the densest plane, which is why FCC slips on {111}.

BCC (100): square of side a = 4R/√3, area 16R²/3. Atoms = 4 × ¼ = 1. PD = 3/(16R²) = 0.1875/R²

BCC (110): rectangle a × a√2, area √2a² = 16√2R²/3. Atoms = 4 × ¼ + 1 (centre) = 2. PD = 3/(8√2R²) = 0.265/R². This is the densest BCC plane.

Numbers for Cu (R = 0.128 nm): PD(110) = 1/(4√2 × 0.01638) = 10.8 atoms/nm² = 1.08 × 10¹⁹ m⁻²; PD(100) = 15.3 nm⁻²; PD(111) = 17.6 nm⁻².
Fe BCC (R = 0.124 nm): PD(110) = 17.2 nm⁻² = 1.72 × 10¹⁹ m⁻²; PD(100) = 12.2 nm⁻².

Linear density

FCC [110] (face diagonal, length 4R): atoms = ½ + 1 + ½ = 2 → LD = 2/4R = 1/(2R). For Cu: 1/(0.256 nm) = 3.91 nm⁻¹.
FCC [100] (edge, length a = 2√2R): 2 × ½ = 1 atom → LD = 1/(2√2R).
BCC [111] (body diagonal, 4R): 2 atoms → LD = 1/(2R). BCC [100]: LD = 1/a = √3/(4R).
Close-packed directions: FCC ⟨110⟩ and BCC ⟨111⟩, where LD = 1/2R (atoms touch).

Interplanar spacing and Bragg's law (X-ray diffraction) Asked: End Sem 2024

When X-rays of wavelength λ (comparable to atomic spacing, ~0.1 nm) hit a crystal, each set of parallel planes (spacing d) scatters them. The reflected waves from successive planes reinforce each other (constructive interference) only when their extra path length, 2d sin θ, equals a whole number of wavelengths.

dθextra path = 2d sin θincident X-rays (λ)diffracted (in phase)nλ = 2d sin θd = a / √(h²+k²+l²)(cubic crystals)2θ = diffraction angle
Derivation of Bragg's law: the ray reflected from the lower plane travels an extra 2 × d sin θ.
Bragg's law and d-spacing
nλ = 2 dhkl sin θ (n = order of reflection, usually 1)
dhkl = a / √(h² + k² + l²) (cubic)

Uses: identifying crystal structure, measuring lattice parameter, finding phases and residual stresses. θ = Bragg angle; diffractometers report 2θ.

Reflection rules: SC: all planes. BCC: h + k + l even (110, 200, 211, 220…). FCC: h, k, l all odd or all even (111, 200, 220, 311…).

Worked numerical 5: d-spacing and diffraction angle

(a) BCC Fe, (220) planes, a = 0.2866 nm, λ = 0.1790 nm, n = 1.

d220 = 0.2866/√(4+4+0) = 0.2866/2.828 = 0.1013 nm

sin θ = nλ/(2d) = 0.1790/(2 × 0.1013) = 0.8833 → θ = 62.04°. Diffraction angle 2θ = 124.1°

(b) FCC Al, (111) planes, a = 0.4049 nm, Cu Kα λ = 0.1542 nm, n = 1.

d111 = 0.4049/√3 = 0.2338 nm; sin θ = 0.1542/(2 × 0.2338) = 0.3298 → θ = 19.26°, 2θ = 38.5°

(c) Reverse problem: for a cubic metal, (211) diffracts at 2θ = 82.4° with λ = 0.1542 nm. θ = 41.2°, sin θ = 0.6587, d = 0.1542/(2 × 0.6587) = 0.1170 nm, a = d√6 = 0.2867 nm (this is α-Fe).

4. Crystal imperfections (defects) High

A real crystal is never perfect. Imperfections are departures from the perfect periodic arrangement. Many properties are structure-sensitive, i.e. controlled by defects: yield strength, ductility, conductivity, diffusion, corrosion. Defects are classified by their dimension:

ClassDimensionExamples
Point defects0-Dvacancy, self-interstitial, substitutional and interstitial impurity, Frenkel, Schottky
Line defects1-Dedge, screw and mixed dislocations
Surface (planar) defects2-Dexternal surface, grain boundaries, twin boundaries, stacking faults, phase boundaries
Volume (bulk) defects3-Dpores, cracks, voids, inclusions, precipitates

4.1 Point defects

VacancySelf-interstitialInterstitial impuritySubstitutional (larger)Substitutional (smaller)
Point defects in a metal.
Schottky: cation + anion vacancy pairFrenkel: cation → interstitial● cation (small) ○ anion (large) ▢ vacancy — ionic solids (NaCl, AgBr); stay neutral.
Hume-Rothery rules (substitutional solid solubility)

Extensive substitutional solubility needs: (1) atomic radius difference < ±15 %; (2) the same crystal structure; (3) similar electronegativity; (4) similar valence. Example: Cu–Ni satisfies all four, so they are completely soluble.

Equilibrium number of vacancies
Nv = N exp(−Qv / kT) N = NA ρ / A

N = atomic sites per unit volume, Qv = energy to form a vacancy, k = 8.62 × 10⁻⁵ eV/atom·K (= 1.38 × 10⁻²³ J/atom·K), T in kelvin. Convert N to m⁻³: multiply atoms/cm³ by 10⁶.

Worked numerical 6: number of vacancies Asked: End Sem 2024

(a) Cu at 200 °C. Qv = 0.9 eV/atom, ρ = 8.94 g/cm³, A = 63.55 g/mol.

Step 1: N = NAρ/A = (6.022 × 10²³ × 8.94)/63.55 = 8.47 × 10²² atoms/cm³ = 8.47 × 10²⁸ atoms/m³

Step 2: T = 200 + 273 = 473 K; kT = 8.62 × 10⁻⁵ × 473 = 0.04077 eV; Qv/kT = 0.9/0.04077 = 22.07

Step 3: Nv = 8.47 × 10²⁸ × e−22.07 = 8.47 × 10²⁸ × 2.59 × 10⁻¹⁰ = 2.2 × 10¹⁹ vacancies/m³

(b) Cu at 1000 °C (ρ = 8.4 g/cm³ at that temperature): N = 7.96 × 10²⁸ m⁻³; T = 1273 K; Qv/kT = 0.9/0.1097 = 8.20; Nv = 7.96 × 10²⁸ × 2.74 × 10⁻⁴ = 2.2 × 10²⁵ vacancies/m³. Raising T from 473 K to 1273 K increases vacancies by about a million times.

(c) Reverse: to find Qv from a given Nv/N, use Qv = −kT ln(Nv/N).

4.2 Line defects: dislocations and the theory of dislocation

Definition

A dislocation is a linear defect around which some atoms are misaligned. It forms the boundary between the slipped and unslipped regions of a crystal. Its magnitude and direction of lattice distortion are given by the Burgers vector b.

Why dislocations were proposed (theory of dislocation)

slip planeextra half-planeAbove slip plane: compression · Below: tension. ⊥ = dislocation line (into page).b ⊥ dislocation lineBurgers vector
Edge dislocation: an extra half-plane of atoms (accent) ends inside the crystal. The line runs perpendicular to the page at ⊥.
Perfect crystal: circuit closes(a) Perfect latticeb (closure failure)⊥Same steps around ⊥ fail to close(b) Lattice with edge dislocation
Burgers circuit. Taking the same number of atom-to-atom steps around the dislocation fails to close. The closure vector is b.
dislocation linebFront-right part sheared by b; step dies out at the line. b ∥ line.● below · ○ above slip planeTop view of slip plane
Screw dislocation: the crystal is sheared by one atomic spacing. The atomic planes form a spiral ramp around the dislocation line, and b is parallel to the line.

Edge vs screw dislocation Asked: End Sem 2024

FeatureEdge dislocationScrew dislocation
DescriptionExtra half-plane of atoms inserted, ending inside the crystalPart of the crystal shifted by one atomic distance; planes form a helical ramp
Burgers vector vs lineb ⊥ dislocation lineb ∥ dislocation line
Direction of motionMoves parallel to b (in the direction of shear stress)Moves perpendicular to b (and to the applied shear)
Slip planeUnique, defined by b and the lineNot unique, so it can cross-slip
Climb (non-conservative motion)Possible, by adding or removing vacancies at high TNot possible
Stress fieldCompressive above, tensile below the slip planePure shear strain
Symbol⊥ (positive), ⊤ (negative)↻ / ↺ (right- or left-handed spiral)
Interaction with solutesStrong: solutes collect in the tensile or compressive region (Cottrell atmosphere → yield point)Weak

Mixed dislocation: most real dislocations are curved, with an edge character at one end and a screw character at the other. b stays constant along the whole line.

Burgers vector magnitude: FCC b = (a/2)⟨110⟩, |b| = a/√2. BCC b = (a/2)⟨111⟩, |b| = a√3/2. HCP b = (a/3)⟨11 2̄ 0⟩, |b| = a. b always lies along the close-packed direction.

4.3 Surface (interfacial) defects

Each grain = a crystal with its ownlattice orientation (hairlines).Thick lines = grain boundaries:disordered, ~2–3 atoms wide,higher energy; block dislocations.Low-angle (<15°) boundary = array ofedge dislocations (tilt) or screwdislocations (twist).
A polycrystal: grains with different lattice orientations, separated by grain boundaries.
Grain size: Hall–Petch and ASTM number
σy = σ0 + ky d−1/2 N = 2n−1

d = average grain diameter. A finer grain size gives higher yield strength and higher toughness. Grain refinement is the only strengthening method that improves both. N = grains per square inch at 100× magnification; n = ASTM grain size number.

Worked numerical 7: Hall–Petch and ASTM

An alloy has σ0 = 70 MPa and ky = 0.74 MPa·m½. For d = 0.01 mm = 1 × 10⁻⁵ m: d−½ = 316.2 m−½, so σy = 70 + 0.74 × 316.2 = 304 MPa. Halving d to 5 µm gives σy = 70 + 0.74 × 447.2 = 401 MPa.

ASTM n = 6 → N = 2⁵ = 32 grains/in² at 100×. If 45 grains/in² are counted at 100×: n = 1 + log 45/log 2 = 1 + 5.49 = 6.5.

4.4 Imperfections: a 5-mark answer outline

Model answer: "Discuss imperfections in crystals in detail" (5 marks)
  1. Definition: any deviation from perfect periodic atomic arrangement. Properties such as strength, ductility, conductivity and diffusion depend on defects.
  2. Classification by dimension (draw the table): point, line, surface, volume.
  3. Point defects: vacancy (equation Nv = N e−Qv/kT), interstitial, substitutional, Schottky and Frenkel. Draw the point-defect sketch.
  4. Line defects: edge (b ⊥ line) and screw (b ∥ line) with sketches. Dislocations explain why real strength is much less than theoretical, and their motion is plastic deformation.
  5. Surface defects: grain boundaries (Hall–Petch), twin boundaries, stacking faults, external surfaces.
  6. Volume defects: voids, cracks, inclusions.
  7. Significance: controlled defects are useful (alloying, strengthening); uncontrolled ones (cracks, pores) cause failure.

5. Plastic deformation: slip and twinning High

Slip

Slip is plastic deformation by the motion of dislocations, which makes one part of the crystal glide over another along specific slip planes in specific slip directions. A slip system = slip plane + slip direction. Slip occurs on the most densely packed plane along the most densely packed direction, because there the atoms move the smallest distance and the planes are farthest apart.

StructureSlip planeSlip directionNo. of slip systemsDuctility
FCC (Cu, Al, Ni){111}⟨1 1̄ 0⟩4 planes × 3 = 12High
BCC (α-Fe, W, Mo){110}, {211}, {321}⟨1̄ 1 1⟩12 + 12 + 24 = 48Moderate (needs higher stress)
HCP (Zn, Mg, Ti)(0001) basal⟨11 2̄ 0⟩1 × 3 = 3Low, brittle in polycrystals

At least 5 independent slip systems are needed for a polycrystal to deform plastically (von Mises). That is why HCP metals are less ductile.

Resolved shear stress and Schmid's law

FFslip planenormal to slip planeslip directionφλτR = σ cos φ cos λφ = angle between F and slip-plane normalλ = angle between F and slip directionYield when τR reaches τCRSSMax Schmid factor = 0.5 at φ = λ = 45°
Worked numerical 8: resolved shear stress

A BCC single crystal is loaded in tension along [010]. Slip is on (110) in the [1̄11] direction.

cos φ: angle between [010] and the plane normal [110] → cos φ = (0·1 + 1·1 + 0·0)/(1 × √2) = 0.707 (φ = 45°)

cos λ: angle between [010] and [1̄11] → cos λ = (0·(−1) + 1·1 + 0·1)/(1 × √3) = 0.577 (λ = 54.7°)

(a) At σ = 52 MPa: τR = 52 × 0.707 × 0.577 = 21.2 MPa

(b) If τCRSS = 30 MPa: σy = 30/(0.707 × 0.577) = 73.5 MPa

Angle between two directions [u₁v₁w₁] and [u₂v₂w₂]: cos θ = (u₁u₂ + v₁v₂ + w₁w₂)/(√(u₁²+v₁²+w₁²) √(u₂²+v₂²+w₂²)).

Twinning

Twinning is plastic deformation in which a shear force moves atoms in a region of the crystal so that this region becomes a mirror image of the parent lattice across a plane called the twin plane. Each atom moves a distance proportional to its distance from the twin plane, always a fraction of an atomic spacing. It happens in BCC and HCP metals at low temperature or high strain rate (shock), when slip is difficult.

SlipBlocks shift by whole atomicspacings → steps (slip bands)twin planetwin planeTwinningAtoms in the twinned band shift in proportion to theirdistance from the twin plane → mirror-image lattice
Slip makes steps of whole atomic spacings. Twinning reorients a band of crystal into a mirror image.

Slip vs twinning

SlipTwinning
Atoms move whole multiples of the interatomic distanceAtoms move fractions of the interatomic distance, proportional to distance from the twin plane
Orientation of the slipped region is unchangedTwinned region becomes a mirror image with a different orientation
Occurs on widely spread planes (slip lines/bands)Occurs in a definite region between twin planes
Needs a lower shear stressNeeds a higher shear stress
Relatively slow (ms)Very fast (µs); may produce an audible "click" (tin cry)
Main mechanism in FCC and BCC; gives large strainsCommon in HCP, and in BCC at low T or impact; gives small strains but reorients grains to favour slip
Slip lines seen under the microscope disappear on polishingTwin bands remain visible after polishing and etching (different orientation)

6. Cold working and hot working Medium

Cold working is plastic deformation below the recrystallization temperature (TR), usually at room temperature. Hot working is deformation above TR.

Strain (work) hardening

During cold work the dislocation density rises from about 10⁶ to 10¹⁰ mm⁻². The dislocations tangle and their strain fields repel each other, so further motion needs more stress. The metal becomes stronger and harder but less ductile.

Percent cold work
%CW = (A0 − Ad) / A0 × 100

A0 = original cross-section area, Ad = area after deformation. For round bars %CW = [1 − (dd/d0)²] × 100.

Worked numerical 9: % cold work

A Cu rod is drawn from 15.2 mm to 12.2 mm diameter. %CW = [1 − (12.2/15.2)²] × 100 = (1 − 0.644) × 100 = 35.6 %. From Callister Fig. 7.19 this gives a yield strength of about 300 MPa, compared with about 70 MPa when annealed.

Thickness reduction of a sheet from 10 mm to 7 mm (width constant): %CW = (10 − 7)/10 × 100 = 30 %.

% cold work →Strength (MPa)Tensile strengthYield strength% cold work →Ductility (%EL)Ductility falls sharply
Effect of cold work: yield and tensile strength (and hardness) rise; ductility falls. Yield strength rises faster, so it approaches tensile strength.

Effects of cold working on properties: ↑ yield strength, ↑ tensile strength, ↑ hardness; ↓ ductility (%EL, %RA), ↓ impact toughness; ↓ electrical conductivity (slightly); ↓ corrosion resistance (stored energy); residual stresses; directional (anisotropic) properties from elongated grains and texture; good surface finish and close tolerances.

BasisCold workingHot working
TemperatureBelow TR (usually room temp.)Above TR
Strain hardeningYes: strength and hardness ↑, ductility ↓No: recrystallization happens at the same time, so the metal stays soft
Grain structureGrains elongated and distortedRefined, equiaxed new grains
Force / energy neededHighLow (larger deformation possible)
Surface finish and accuracyExcellent, close tolerancesPoor (oxide scale), lower accuracy
Residual stressesPresent; need stress-relief annealingNegligible
DefectsMay crack if overworkedCloses porosity, breaks up the cast structure, removes inhomogeneity
ExamplesCold rolling, wire drawing, deep drawing, coiningHot rolling, forging, extrusion, piercing

7. Recovery, recrystallization and grain growth High

A cold-worked metal stores strain energy (dislocations, point defects). On annealing (heating) it softens in three stages:

Annealing temperature →Strength / DuctilityRecoveryRecrystallizationGrain growthTensile strengthDuctilityT_R ≈ 0.3–0.5 T_m (K)Grain sizecoarsenew fine, strain-free grainscold-worked (deformed) grains
Effect of annealing temperature on a cold-worked metal (fixed time, e.g. 1 h).

(1) Recovery

(2) Recrystallization

(3) Grain growth

Grain growth law
dⁿ − d0ⁿ = K t (n ≈ 2; K rises exponentially with temperature)
RecoveryRecrystallizationGrain growth
TemperatureLow (< TR)≈ TR (0.3–0.5 Tm)> TR
MicrostructureNo visible change; polygonizationNew equiaxed strain-free grainsGrains coarsen
Strength / hardnessSlight decreaseLarge decreaseSmall further decrease
DuctilitySlight increaseLarge increaseSlight increase / constant
Residual stressRelievedFully removed—
Driving forceStored dislocation energyStored strain energyGrain-boundary energy

Further reading: Callister Ch. 3 (structures, Miller indices, XRD §3.16), Ch. 4 (imperfections), Ch. 7 (dislocations, slip, strengthening, recovery and recrystallization §7.10–7.13).

Likely exam questions (Unit 1)

#QuestionMarks
1Define APF and coordination number. Derive APF for SC, BCC and FCC (and HCP).4–5
2Derive the relation between a and R for SC, BCC and FCC with neat sketches.3
3Calculate the planar density of FCC (110) (or (100), (111)) and BCC (110) in terms of R.3–4
4State Bragg's law. For BCC Fe find d220 and the diffraction angle (a = 0.2866 nm, λ = 0.1790 nm, n = 1).3–4
5Tabulate the axial relationships and inter-axial angles of the seven crystal systems.2–3
6Explain the procedure to find Miller indices of planes and directions in cubic and HCP crystals with examples. Convert [010] and [111] to Miller–Bravais indices.5
7What is a single crystal? Discuss crystal imperfections in detail.5
8Compute the number of vacancies per m³ in Cu at 200 °C (Qv = 0.9 eV/atom, ρ = 8.94 g/cm³, A = 63.55).3
9Differentiate between edge and screw dislocations with sketches. Define Burgers vector.4
10Differentiate between slip and twinning. Why are FCC metals more ductile than HCP?4
11Explain recovery, recrystallization and grain growth with a property-vs-temperature diagram. What factors affect recrystallization temperature?5
12Compare cold working and hot working. Explain the effect of cold work on mechanical properties.4
Model answer: why FCC is more ductile than BCC and HCP (2–3 marks)

Ductility needs many active slip systems on close-packed planes. FCC has 12 slip systems on truly close-packed {111} planes (PD = 0.289/R²) along ⟨110⟩, with a low Peierls stress, so dislocations move easily even at very low temperatures. BCC has 48 systems, but none of its planes is truly close-packed, so it needs a higher, temperature-sensitive stress and shows a ductile–brittle transition. HCP has only 3 basal slip systems, fewer than the 5 independent systems needed for polycrystal plasticity, so it is the least ductile.

Model answer: single crystal vs polycrystal (2 marks)

A single crystal has a continuous, unbroken periodic lattice through the whole specimen with no grain boundaries, so its properties are anisotropic (e.g. E of Fe is 273 GPa along [111] and 125 GPa along [100]). A polycrystal consists of many randomly oriented grains separated by boundaries, so its properties are averaged and nearly isotropic. Uses of single crystals: Si wafers for ICs, Ni-superalloy turbine blades (no grain boundaries means better creep resistance), piezoelectric quartz.

Model answer: Miller indices of a plane, worked in the exam layout (3 marks)

Plane intercepts: x = 1, y = ½, z = ⅓. Reciprocals: 1, 2, 3. No fractions to clear → (123). Sketch: mark the points (1,0,0), (0,½,0), (0,0,⅓) in the cube and join them into a triangle. For a plane through the origin, first shift the origin to an adjacent corner, then repeat the steps.

Unit 2 · ~8 contact hrs

Engineering Materials & Corrosion

Most asked: composition, properties and uses of duralumin, brasses and bronzes (2-mark table); effect of alloying elements; stainless-steel types; galvanic cell and rusting of iron; methods of corrosion protection.
How this unit is examined

This unit is mostly theory. Expect short parts (2–3 marks): "composition, properties and applications of duralumin / brass", "effect of Ni, Cr, Mo in steel", and one 4–5 mark corrosion part (mechanism of rusting, galvanic cell, protection methods). Learn the alloy table in §5 and the rusting reactions word-perfect.

1. Plain carbon steels High

Definition

Plain carbon steel is an alloy of iron and carbon (up to 2.11 % C, practically ≤ 1.5 %). Its properties are controlled mainly by carbon. It contains only small residual amounts of Mn (≤ 1.0 %), Si (≤ 0.4 %), S and P (each ≤ 0.05 %), and no deliberately added alloying element.

Classification by carbon content

Type% CMicrostructure (annealed)PropertiesApplications
Dead-mild steel< 0.15almost all ferritevery soft, very ductile, excellent weldability and formabilitywires, thin sheets, rivets, nails, tubes, car body panels
Low-carbon (mild) steel0.15–0.30ferrite + some pearliteUTS ~ 400 MPa, ductile, tough, weldable, machinable; cannot be hardened by quenchingstructural sections (I-beams, angles), bridges, ship plates, nuts and bolts, pipes, case-carburized gears
Medium-carbon steel0.30–0.60ferrite + pearlite (~ 50 %)stronger, harder; good balance of strength and toughness; can be hardened and temperedshafts, axles, crankshafts, connecting rods, gears, rails, forgings, machine parts
High-carbon steel0.60–0.80mostly pearlitehigh strength and hardness, wear resistant, low ductilitysprings, wire ropes, hammers, chisels, punches, rail wheels
Tool (very high-C) steel0.80–1.5pearlite + proeutectoid cementitevery hard, wear resistant, brittle; poor weldabilityfiles, razors, drills, taps, knives, wood-working tools, ball bearings
Property (relative)Carbon content (wt%) →00.20.40.60.81.01.21.4UTS (peaks ≈ 0.8–1.0 %C)Hardness (keeps rising)Ductility / %EL / impact toughness / weldability0.76 eutectoid
Effect of carbon on the properties of annealed plain carbon steel. UTS peaks near the eutectoid region because a continuous cementite network forms at the grain boundaries above about 1 % C.

Role of residual elements

Designation: AISI/SAE 10xx, where xx = %C × 100 (1020 = 0.20 % C, 1045 = 0.45 % C, 1080 = 0.80 % C). Indian IS: 40C8 = 0.40 % C, 0.8 % Mn; also C45.

Limitations of plain carbon steels (why we alloy)

  1. Low hardenability: they need a drastic water quench, which causes distortion and quench cracks, and thick sections do not harden through.
  2. Strength above about 700 MPa is only possible with a large loss of ductility and toughness.
  3. Poor corrosion and oxidation resistance.
  4. Lose strength and creep resistance at high temperatures; soften quickly on tempering.
  5. Poor impact toughness at low temperatures (ductile–brittle transition).

2. Effect of alloying elements High

An alloy steel contains deliberately added elements (Ni, Cr, Mo, W, V, Mn > 1 %, Si > 0.5 %…) to improve properties. Low-alloy steels have < 5 % total alloy; high-alloy steels have > 5–10 % (stainless, tool, Hadfield).

General effects

  1. Increase hardenability: they shift the TTT curve to the right (slower transformation), so martensite forms even on oil or air cooling and thick sections harden through. Co is the exception: it shifts the curve to the left.
  2. Change the phase diagram:
    • Austenite (γ) stabilizers: Ni, Mn, C, N, Cu, Co. They lower A₁/A₃ and widen the γ field (enough Ni or Mn gives austenitic steel at room temperature).
    • Ferrite (α) stabilizers: Cr, Si, Mo, W, V, Ti, Al, Nb. They raise A₃ and shrink the γ loop.
    • Almost all alloying elements shift the eutectoid point to lower carbon.
  3. Form carbides: Ti, Nb, V, W, Mo, Cr (in decreasing tendency) form hard carbides, which add wear resistance and hot hardness. Ni, Si, Al and Co do not form carbides (they are graphitizers).
  4. Solid-solution strengthening of ferrite (Si, Mn, Ni, P).
  5. Grain refinement (V, Ti, Nb, Al), which gives better toughness.
  6. Resistance to tempering and secondary hardening (Mo, W, V, Cr), so the steel keeps its hardness at high temperature.
  7. Lower Ms and Mf, which may leave retained austenite.
  8. Corrosion and oxidation resistance (Cr ≥ 11–12 %, Ni, Cu, Si, Al).

Element-wise effects (learn at least Ni, Cr, Mn, Si, Mo, W, V)

ElementMain effectsTypical use
Nickel (Ni)γ-stabilizer; raises strength and toughness, especially at low temperature; raises hardenability; with Cr gives corrosion resistance; refines grainNi–Cr–Mo steels (4340), 18-8 stainless, cryogenic 9 % Ni steel
Chromium (Cr)α-stabilizer, carbide former; raises hardenability, wear resistance and high-temperature strength; > 11–12 % gives corrosion resistance (passive Cr₂O₃ film)bearing steel 52100 (1.5 % Cr), stainless, tool steels
Manganese (Mn)deoxidizer and desulphurizer (MnS, prevents hot shortness); raises strength and hardenability; γ-stabilizer; 12 % Mn gives austenitic wear-resistant steelall steels; Hadfield steel
Silicon (Si)deoxidizer; strengthens ferrite; raises elastic limit (spring steels, 1.5–2 % Si); 3–4 % Si raises electrical resistivity and magnetic permeability and lowers hysteresis loss; graphitizerSi–Mn spring steel, transformer (electrical) steel
Molybdenum (Mo)raises hardenability strongly; raises high-temperature strength and creep resistance; reduces temper embrittlement; improves pitting resistance in stainless (316)Cr–Mo boiler steels, HSS (M-series), 316 SS
Tungsten (W)strong carbide former; red hardness (keeps hardness at 550–600 °C); wear resistance; fine grainhigh-speed steel 18-4-1, hot-work dies
Vanadium (V)strongest grain refiner; very hard carbides (VC) for wear resistance; toughness; secondary hardeningHSS, Cr–V tools (spanners), springs
Cobalt (Co)raises red hardness in HSS; lowers hardenability (the only one); magnetic propertiessuper HSS, permanent magnets
Titanium (Ti), Niobium (Nb)very strong carbide formers; grain refiners (micro-alloyed HSLA); stabilize stainless steel against weld decay (321, 347)HSLA steel, stabilized SS
Copper (Cu)0.2–0.5 % improves atmospheric corrosion resistance (weathering steel); precipitation strengtheningCorten steel
Boron (B)only 0.001–0.003 % greatly raises hardenabilityboron steels for bolts
Aluminium (Al)deoxidizer, grain refiner; forms hard AlN in nitriding steelsNitralloy
Lead (Pb), Sulphur (S)improve machinability (chips break easily)free-cutting steels

3. Tool steels Medium

Tool steels are high-quality carbon or alloy steels used to make tools for cutting, forming, shaping and shearing other materials.

Requirements: high hardness; wear resistance; adequate toughness (shock resistance); red / hot hardness (keeps hardness at the high temperature of cutting); good hardenability with minimum distortion; machinability before hardening.

AISI groupTypical compositionKey featureUses
W water-hardening0.6–1.4 C (plain carbon)cheap, hard surface, tough core; low hardenability; loses hardness above 200 °Cfiles, chisels, wood-working tools, hand tools
O oil-hardening (O1)0.9 C, 1.0 Mn, 0.5 Cr, 0.5 Wless distortiongauges, dies, punches, taps
A air-hardening (A2)1.0 C, 5 Cr, 1 Mominimum distortionblanking and forming dies
D high-C high-Cr (D2)1.5 C, 12 Cr, 1 Mo, 1 Vexcellent wear resistancelong-run dies, shear blades, rolls
S shock-resisting (S1)0.5 C, 1.5 Cr, 2.5 Whigh toughnesschisels, punches, rivet sets, pneumatic tools
H hot-work (H13)0.4 C, 5 Cr, 1.3 Mo, 1 Vresists softening and thermal fatigueforging dies, die-casting dies, extrusion dies
T tungsten high-speed (T1 = 18-4-1)0.75 C, 18 W, 4 Cr, 1 Vred hardness to ~ 600 °C; cuts at high speeddrills, lathe tools, milling cutters, broaches
M molybdenum high-speed (M2)0.85 C, 6 W, 5 Mo, 4 Cr, 2 Vcheaper and tougher than T-type; most used HSStwist drills, taps, end mills, saw blades
P mould steels (P20)low C, Cr–Moeasily machined, polishedplastic injection moulds

4. Stainless steels and wear-resistant steels High

Definition

Stainless steels are iron alloys with at least 10.5–12 % Cr. The Cr forms a thin, adherent, self-healing passive film of Cr₂O₃ that protects the metal from corrosion. Ni, Mo, N, Ti and Nb are added to improve particular properties.

TypeCompositionStructurePropertiesGrades and uses
Ferritic12–27 % Cr, < 0.12 % C, no NiBCC ferritemagnetic; not hardenable by heat treatment; good resistance to stress-corrosion cracking; moderate corrosion resistance; cheap430, 409: automobile exhaust and trim, kitchen sinks, washing-machine drums
Martensitic12–18 % Cr, 0.15–1.2 % CBCT martensite after quenchmagnetic; hardenable (Q + T); high strength and hardness; lowest corrosion resistance of the stainless steels410, 420, 440C: cutlery, surgical instruments, valves, turbine blades, ball bearings
Austenitic16–26 % Cr, 6–22 % Ni (18-8), < 0.08 % CFCC austenite (Ni stabilizes γ)non-magnetic; best corrosion resistance; very ductile and tough even at cryogenic temperature; strengthened only by cold work; prone to sensitization304 (18Cr-8Ni), 316 (+2–3 Mo): kitchenware, food, dairy and chemical plant, cryogenic tanks, architecture
Duplex22–25 % Cr, 5–7 % Ni, 3 % Mo, N~ 50 % ferrite + 50 % austeniteabout twice the yield strength of 304; excellent resistance to SCC and pitting; weldable2205: oil and gas, desalination, chemical tankers, heat exchangers
Precipitation-hardening (PH)17 % Cr, 4–7 % Ni + Cu / Al / Nbmartensitic or semi-austenitic + precipitatesvery high strength (up to 1400 MPa) through ageing, with good corrosion resistance17-4 PH, 17-7 PH: aircraft parts, springs, shafts, pump parts
Sensitization (weld decay) in austenitic SS: frequently asked

When 18-8 steel is heated in the range 425–870 °C (e.g. near a weld), chromium carbide Cr₂₃C₆ precipitates along the grain boundaries. The adjacent zone loses Cr below 12 % and is no longer stainless, so intergranular corrosion occurs. Remedies: (1) low-carbon grades (304L, 316L, C < 0.03 %); (2) stabilized grades with Ti (321) or Nb (347), which form TiC/NbC instead of Cr carbide; (3) solution anneal at about 1050 °C and quench to redissolve the carbides.

Wear-resistant steels

5. Non-ferrous alloys: Al, Cu, Zn High

5.1 Aluminium and its alloys

Properties of Al: low density (2.7 g/cm³, about ⅓ of steel); FCC, so ductile and formable with no ductile–brittle transition; high electrical and thermal conductivity (about 60 % of Cu); excellent corrosion resistance from a protective Al₂O₃ film; non-toxic, non-magnetic; low melting point (660 °C); high specific strength in alloys. Limitation: low strength in the pure state, which is improved by alloying, cold work and age (precipitation) hardening.

SeriesMain alloying elementHeat-treatable?Example and uses
1xxx≥ 99 % AlNo1100: foil, electrical conductors, chemical equipment
2xxxCu (+ Mg)Yes2024 / 2017 (duralumin): aircraft structures, rivets, truck wheels
3xxxMnNo3003: cooking utensils, beverage cans, heat exchangers
4xxxSiNowelding filler wire, brazing
5xxxMgNo5052, 5083: marine and ship hulls, pressure vessels
6xxxMg + SiYes6061, 6063: window frames, extrusions, bicycle frames, automobile parts
7xxxZn (+ Mg, Cu)Yes7075: highest strength (about 570 MPa); aircraft wings and spars

5.2 Copper and its alloys

Properties of Cu: excellent electrical and thermal conductivity (second only to Ag); FCC, so very ductile and malleable; good corrosion resistance; non-magnetic; density 8.96 g/cm³; easily joined; attractive colour. Pure Cu (electrolytic tough pitch, ETP, 99.9 %): electrical wiring, bus bars, heat exchangers. Brass = Cu + Zn. Bronze = Cu + Sn (more broadly Cu + any element other than Zn).

Brasses (Cu–Zn)

Bronzes

5.3 Zinc and its alloys

Properties of Zn: HCP; density 7.14 g/cm³; low melting point (419 °C), so it is ideal for die casting; good fluidity; anodic to steel (sacrificial). Recrystallizes at about room temperature, so it cannot be work-hardened. Uses: about half of all Zn goes into galvanizing steel; also brass making, dry-cell cases, sacrificial anodes and roofing sheets.
Zamak die-casting alloys (Zn + 4 % Al + 0.04 % Mg; Zamak 5 adds 1 % Cu): good dimensional accuracy, thin sections, easy plating. Used for carburettor and fuel-pump bodies, door handles, locks, zip fasteners, toys and automobile trim. Zn–22 % Al is superplastic.

5.4 Master table: important non-ferrous alloys Asked: End Sem 2024

AlloyCompositionPropertiesApplications
DuraluminAl + 3.5–4.5 % Cu, 0.4–0.8 % Mg, 0.4–0.7 % Mn, ~ 0.5 % Silight (2.8 g/cm³); age-hardenable (solution treat about 500 °C, quench, age); UTS up to about 400–450 MPa, close to mild steel; good machinability; poorer corrosion resistance (hence Alclad: clad with pure Al)aircraft structures and skins, rivets, automobile and truck parts, surgical and orthopaedic devices, high-speed train bodies
Y-alloyAl + 4 % Cu, 2 % Ni, 1.5 % Mgage-hardenable; keeps strength at high temperature (200–250 °C); good castabilityIC-engine pistons, cylinder heads, crankcases
Brass (general)Cu + Zn (5–45 %)stronger and cheaper than Cu; good corrosion resistance; easily cast, machined and formed; gold-like colourplumbing fittings, valves, radiators, musical instruments, electrical terminals, decorative items
Cartridge brass70 % Cu, 30 % Zn (α)maximum ductility of all brasses; excellent cold formability (deep drawing)cartridge cases, radiator cores, lamp fittings, deep-drawn articles
Muntz metal60 % Cu, 40 % Zn (α + β)stronger and harder, less ductile; good hot-workability; cheapcondenser tube plates, ship sheathing, nuts and bolts, valve stems
Admiralty / naval brass71Cu-28Zn-1Sn / 60Cu-39Zn-1SnSn resists dezincification in seawatercondenser tubes, marine hardware, propeller shafts
Bronze (tin bronze)Cu + 5–20 % Snharder, stronger and more corrosion-resistant than brass; good wear and bearing properties; low frictionbearings, bushes, gears, statues, coins, bells (bell metal ~ 20 % Sn)
Gun metal88 % Cu, 10 % Sn, 2 % Znstrong, tough, pressure-tight castings; good corrosion and wear resistancebearings, valves, pump bodies, steam fittings, gears (historically guns)
Phosphor bronzeCu + 4–11 % Sn + 0.1–0.35 % Phigh strength and elasticity, fatigue and wear resistant, low frictionsprings, bearings, worm wheels, electrical contacts
German silver (nickel silver)~ 60 % Cu, 20 % Zn, 20 % Ni (no silver)silvery-white, corrosion resistant, high electrical resistivitycutlery, utensils, jewellery, musical instruments, resistance wires, keys
Cupronickel70 % Cu, 30 % Ni (75/25 for coins)excellent seawater corrosion resistancemarine condenser tubes, coins
Zamak 3Zn + 4 % Al + 0.04 % Mglow melting point, excellent castabilitydie-cast handles, locks, carburettors
Brass vs bronze (2 marks)
BrassBronze
CompositionCu + ZnCu + Sn (or Al, Si, Be, P)
Colourbright yellow (gold-like)reddish brown
Strength and hardnesslowerhigher
Corrosion resistancegood, but dezincification in seawaterbetter, especially in seawater
Friction and wearmoderatelow friction, so better for bearings
Cost and machinabilitycheaper; excellent machinabilitycostlier (Sn)
Usesfittings, radiators, cartridge casesbearings, bushes, springs, propellers, statues

6. Corrosion: basics and types High

Definition

Corrosion is the destructive and unintentional deterioration of a metal by chemical or electrochemical reaction with its environment. In effect it is extractive metallurgy in reverse: the metal returns to its stable oxide or compound state.

Dry vs wet corrosion

Dry (chemical) corrosionWet (electrochemical) corrosion
Direct chemical attack by gases (O₂, Cl₂, H₂S, SO₂) at high temperature, with no liquid electrolyteNeeds an electrolyte (moisture, seawater, acid); anodic and cathodic areas form
Uniform; the product forms on the spot where attack occursAnode corrodes; the product forms between anode and cathode
Slow; adsorption and diffusion mechanismFast; electrochemical (galvanic cell) mechanism
e.g. oxidation of Fe in a furnace, tarnishing of Age.g. rusting of iron, corrosion of ship hulls

Pilling–Bedworth ratio (dry oxidation): PBR = volume of oxide / volume of metal consumed = Aoxideρmetal / (n Ametal ρoxide). If PBR < 1 (Mg, Na), the oxide is porous and non-protective. If 1–2 (Al, Cr, Ni, Ti), it is protective. If > 2 (Fe), it cracks and spalls off.

Electrochemical basis (wet corrosion)

Four things are needed: an anode, a cathode, an electrolyte, and a metallic path for electrons. Remove any one and corrosion stops (this is the basis of all protection methods).

Reactions
Anode (oxidation, corrodes): M → Mⁿ⁺ + n e⁻
Cathode, acid: 2H⁺ + 2e⁻ → H₂↑ (hydrogen evolution)
Cathode, acid + O₂: O₂ + 4H⁺ + 4e⁻ → 2H₂O
Cathode, neutral/basic + O₂: O₂ + 2H₂O + 4e⁻ → 4OH⁻ (oxygen absorption)
Metal-ion reduction: Mn+ + n e⁻ → M

Galvanic cell High

When two dissimilar metals are electrically connected in an electrolyte, the more active metal (lower, more negative electrode potential) becomes the anode and corrodes. The more noble metal becomes the cathode and is protected. The Daniell cell (Zn–Cu) is the classic example.

ZnSO₄ (1 M)ZnZn anode (−)CuSO₄ (1 M)CuCu cathode (+)salt bridge (KCl)1.10 Ve⁻ →e⁻ →Anode: Zn → Zn²⁺ + 2e⁻ (oxidation, corrodes)Cathode: Cu²⁺ + 2e⁻ → Cu (reduction)
Zn–Cu galvanic cell. Ecell = Ecathode − Eanode = +0.34 − (−0.76) = 1.10 V.
Electrode reactionE° (V)
Au³⁺ + 3e⁻ → Au+1.420
O₂ + 4H⁺ + 4e⁻ → 2H₂O+1.229
Ag⁺ + e⁻ → Ag+0.800
Cu²⁺ + 2e⁻ → Cu+0.340
2H⁺ + 2e⁻ → H₂0.000
Pb²⁺ + 2e⁻ → Pb−0.126
Sn²⁺ + 2e⁻ → Sn−0.136
Ni²⁺ + 2e⁻ → Ni−0.250
Cd²⁺ + 2e⁻ → Cd−0.403
Fe²⁺ + 2e⁻ → Fe−0.440
Zn²⁺ + 2e⁻ → Zn−0.763
Al³⁺ + 3e⁻ → Al−1.662
Mg²⁺ + 2e⁻ → Mg−2.363

Standard EMF series (25 °C, 1 M). Top = noble (cathodic); bottom = active (anodic).

Galvanic series (practical ranking in seawater, including alloys):

More noble (cathodic) ↑
Platinum · Gold · Graphite · Titanium · Silver · 316 SS (passive) · 304 SS (passive) · Inconel / Nickel (passive) · Monel · Cupronickel · Bronzes · Copper · Brasses · Nickel (active) · Tin · Lead · 316 / 304 SS (active) · Cast iron · Iron and steel · Aluminium alloys · Cadmium · Pure aluminium · Zinc · Magnesium and its alloys
↓ More active (anodic)

EMF vs galvanic series: the EMF series is for pure metals in 1 M solutions of their own ions, a theoretical and fixed ranking. The galvanic series covers metals and alloys in a real environment (seawater), and the same alloy can appear in both an active and a passive position.

Nernst equation (non-standard concentrations)
ΔV = (V₂° − V₁°) − (0.0592 / n) log ([M₁ⁿ⁺] / [M₂ⁿ⁺]) (25 °C)

Metal 1 is oxidized (anode); metal 2 is reduced (cathode).

Worked numerical: cell potential

(a) Zn–Cu standard cell: E = 0.340 − (−0.763) = 1.10 V; Zn corrodes.

(b) Ni in 10⁻³ M Ni²⁺ connected to Cd in 0.5 M Cd²⁺. Cd (−0.403) is more active, so Cd is oxidized (metal 1) and Ni²⁺ is reduced (metal 2).
ΔV = (−0.250 − (−0.403)) − (0.0592/2) log (0.5/10⁻³) = 0.153 − 0.0296 × 2.699 = 0.153 − 0.080 = +0.073 V. It is positive, so the reaction is spontaneous as written.

Corrosion penetration rate
CPR = K W / (ρ A t) K = 87.6 → mm/yr (W in mg, ρ in g/cm³, A in cm², t in h)

Worked: a steel sheet (ρ = 7.9) of area 400 cm² loses 375 g in 1 year (8760 h). CPR = 87.6 × 375 000/(7.9 × 400 × 8760) = 1.19 mm/yr.

Rusting of iron: mechanism High

Rusting is the electrochemical corrosion of iron in the presence of both water and oxygen. Different parts of the same iron surface act as anode and cathode (impurities, stresses, or differential aeration). Under a water drop, the centre (poor in O₂) becomes the anode and the edge (rich in O₂) becomes the cathode.

Iron / steelwater drop (electrolyte)Fe²⁺ + 2OH⁻ → Fe(OH)₂ → Fe(OH)₃ → rust ringFe → Fe²⁺ + 2e⁻Anode (centre, low O₂)O₂ from airO₂ from aire⁻ flow in metalCathodes at the rim (O₂-rich): O₂ + 2H₂O + 4e⁻ → 4OH⁻
Differential-aeration cell under a water drop on iron.
Reactions (write all of them)
Anode: Fe → Fe²⁺ + 2e⁻ (×2)
Cathode: O₂ + 2H₂O + 4e⁻ → 4OH⁻
Overall: 2Fe + O₂ + 2H₂O → 2Fe²⁺ + 4OH⁻ → 2Fe(OH)₂ (ferrous hydroxide, greenish)
Further oxidation: 4Fe(OH)₂ + O₂ + 2H₂O → 4Fe(OH)₃ (ferric hydroxide)
Dehydration: 2Fe(OH)₃ → Fe₂O₃·xH₂O (rust, reddish brown, hydrated ferric oxide)

In acidic water the cathode reaction is 2H⁺ + 2e⁻ → H₂ (hydrogen evolution). Rust is porous and non-adherent (PBR > 2), so it does not protect the iron underneath and attack continues. Salt water corrodes faster because it is a better electrolyte.

Forms (types) of corrosion

TypeDescription and causeExamplePrevention
Uniform attackEven corrosion over the whole exposed surface; most common, predictablerusting of steel sheet, tarnish on silvercoatings, corrosion allowance, inhibitors
Galvanic (bimetallic)Two dissimilar metals in contact in an electrolyte; the more active one corrodes. A small anode with a large cathode is very dangeroussteel bolts in copper plate, Zn–Cuchoose metals close in the galvanic series; insulate joints; large anode area; coat the cathode
CreviceConcentration (O₂-depletion) cell in narrow gaps, under gaskets, washers and depositsunder rivet heads, bolt washerswelded joints instead of riveted; non-absorbing gaskets; avoid stagnant areas
PittingLocalized attack forming small deep pits; autocatalytic; very dangerous because it is hard to detectstainless steel in chloride (seawater)add Mo (316 SS); polish surfaces; avoid Cl⁻
IntergranularAttack along grain boundaries because of Cr depletion (sensitization)weld decay of 18-8 SSlow-C (L grades), Ti/Nb stabilization, solution anneal
Selective leachingOne element of an alloy is removed preferentiallydezincification of brass; graphitic corrosion of cast ironAs/Sb/P or Sn additions; change alloy
Erosion–corrosionCombined chemical attack and mechanical abrasion by a fast-moving fluid that removes the protective filmpipe elbows, pump impellers, propellersreduce velocity and turbulence; streamlined design; harder alloys
Stress corrosion cracking (SCC)Cracking under tensile stress (applied or residual) together with a specific corrosive environmentbrass in ammonia (season cracking); SS in hot chloridesstress-relief anneal; lower stress; change environment; duplex SS
Hydrogen embrittlementAtomic H diffuses into steel and lowers ductility, causing brittle failurehigh-strength steel during pickling or electroplatingbake at about 200 °C; lower-strength steel; avoid H sources

Factors affecting the rate of corrosion

7. Methods of protection from corrosion High

  1. Proper selection of material: use noble or passive metals (SS, Ti, Cu alloys) or non-metals (plastics, ceramics) where economical. Use pure, homogeneous metal.
  2. Proper design:
    • avoid contact of dissimilar metals, or insulate them (gaskets, washers);
    • if contact is unavoidable, make the anode area large and the cathode small;
    • avoid crevices (weld rather than rivet), sharp corners and stagnant pockets;
    • provide drainage; allow easy inspection, cleaning and replacement;
    • add a corrosion allowance to the thickness; avoid residual stresses (stress-relieve).
  3. Modifying the environment: lower the temperature and fluid velocity; remove O₂ (deaeration with hydrazine or Na₂SO₃ in boiler water); dehumidify; neutralize acids; add inhibitors.
    • Anodic inhibitors (chromates, phosphates, nitrites) form a passive film on the anode.
    • Cathodic inhibitors (Zn, Mg and Ni salts, organic amines) block the cathode reaction.
    • Vapour-phase inhibitors are used for packaging.
  4. Protective coatings:
    • Metallic, anodic coatings: coating metal more active than the base, e.g. galvanizing (Zn on steel, hot dip at about 450 °C) or cadmium plating. They protect even when scratched.
    • Metallic, cathodic coatings: a nobler metal, e.g. tinning (Sn on steel), Ni or Cr plating. They protect only while unbroken.
    • Methods of applying: hot dipping, electroplating, metal spraying, cladding (Alclad), cementation (sherardizing with Zn powder, calorizing with Al, chromizing).
    • Inorganic / chemical conversion coatings: anodizing (thick Al₂O₃ on Al), phosphating (Fe/Zn phosphate under paint, e.g. car bodies), chromating, enamelling.
    • Organic coatings: paints (red-lead or zinc-chromate primer + top coat), varnishes, lacquers, epoxy, rubber and plastic linings.
  5. Cathodic protection: make the structure the cathode so that it cannot corrode.
    • Sacrificial anode method: a more active metal (Mg, Zn, Al) is connected to the structure and corrodes instead. It is replaced periodically. Used for buried pipelines, ship hulls, water heaters and offshore platforms.
    • Impressed current method: a DC supply makes the structure the cathode, with an inert anode (graphite, high-Si iron, Pt-coated Ti) in the soil or water. Used for long pipelines, tanks and large structures.
  6. Anodic protection and passivation: for metals that passivate (SS, Ti), applying an anodic potential or using oxidizing acids (HNO₃) keeps a stable passive film.
(a) Sacrificial anodeSteel pipe (cathode)Mg / Zn(anode, corrodes)wiresoil / sea water(b) Impressed currentTank / pipe (−)inert anode (+)DC−+
Cathodic protection: (a) sacrificial anode; (b) impressed current.
Galvanised (Zn on Fe)FeZnscratchZn corrodes, Fe protectedTinned (Sn on Fe)FeSnscratchFe corrodes fast (pit)
When the coating is scratched, Zn (anodic) protects the steel sacrificially. Sn (cathodic) makes the exposed steel a small anode next to a large cathode, so it pits rapidly.
GalvanizingTinning
Coating of Zn on steel (hot dip in molten Zn at about 450 °C)Coating of Sn on steel (hot dip at about 230 °C or electrolytic)
Zn is anodic to Fe, giving sacrificial protectionSn is cathodic to Fe, giving barrier protection only
Protects Fe even if the coating is scratched or brokenIf scratched, Fe corrodes faster than uncoated steel
Zn dissolves in dilute acids and is toxic, so not used for foodSn is non-toxic, so used for food cans and containers
Uses: roofing sheets, pipes, buckets, wires, fencingUses: food cans, utensils, copper wires (for soldering)

Further reading: Callister Ch. 11 (ferrous and non-ferrous alloys §11.2–11.3), Ch. 17 (corrosion §17.2–17.9).

Likely exam questions (Unit 2)

#QuestionMarks
1Give the composition, properties and applications of (a) duralumin (b) brass (or gun metal, Y-alloy, German silver, Muntz metal).2–3
2Classify plain carbon steels. Give the properties and uses of each class. What are their limitations?4
3Discuss the effect of alloying elements (Ni, Cr, Mo, W, V, Mn, Si) on the properties of steel.4–5
4What are stainless steels? Classify them and give the composition, properties and applications of each. What is weld decay and how is it prevented?5
5Write short notes on (a) Hadfield manganese steel (b) high-speed steel (c) tool steels.3
6Differentiate between brass and bronze. Explain dezincification.3
7Explain the electrochemical mechanism of rusting of iron with reactions.4
8What is a galvanic cell? Distinguish between the EMF series and the galvanic series.3–4
9Describe the various forms of corrosion with examples.5
10Discuss methods of corrosion protection. Explain cathodic protection. Compare galvanizing and tinning.5
Model answer: duralumin and brass (2 marks, "Asked: End Sem 2024" type)

Duralumin: Al + 4 % Cu + 0.5 % Mg + 0.5 % Mn (+ 0.5 % Si). Light (2.8 g/cm³), age-hardenable to about 400 MPa (close to mild steel), good machinability, moderate corrosion resistance (clad with pure Al as Alclad). Uses: aircraft structures, rivets, automobile parts, surgical instruments.
Brass: Cu + Zn, e.g. cartridge brass 70Cu–30Zn and Muntz metal 60Cu–40Zn. Good strength and ductility, corrosion resistant, easily cast, machined and deep-drawn, attractive yellow colour. Uses: cartridge cases, radiator cores, plumbing fittings, valves, musical instruments, condenser plates.

Model answer: mechanism of rusting (4 marks)

Rusting is electrochemical (wet) corrosion of iron that needs both water and O₂. A differential-aeration cell forms: the region with less O₂ (e.g. the centre of a water drop) becomes the anode and the O₂-rich region becomes the cathode. Draw the water-drop figure.
Anode: Fe → Fe²⁺ + 2e⁻. Cathode: O₂ + 2H₂O + 4e⁻ → 4OH⁻. Fe²⁺ + 2OH⁻ → Fe(OH)₂; 4Fe(OH)₂ + O₂ + 2H₂O → 4Fe(OH)₃; Fe(OH)₃ → Fe₂O₃·xH₂O (rust).
Rust deposits between the anode and cathode. It is porous (PBR > 2), so attack continues. Salt and acids accelerate rusting. Prevented by paint, galvanizing and cathodic protection.

Model answer: effect of Ni, Cr and Mo (3 marks)

Ni: austenite stabilizer; raises toughness (especially at low temperature), strength and hardenability; with Cr, gives austenitic stainless steel. Cr: carbide former; raises hardenability, wear resistance and high-temperature strength; ≥ 12 % gives corrosion resistance through a passive Cr₂O₃ film. Mo: raises hardenability and creep strength, prevents temper embrittlement, adds red hardness in HSS and pitting resistance in 316 SS.

Unit 3 · ~8 contact hrs

Solidification, Phase Diagrams & Heat Treatment

Most examined: the Fe–Fe₃C diagram and its reactions, the TTT diagram, annealing vs normalizing, Gibbs phase rule and lever-rule numericals. This unit alone can be worth 16 of your 40 marks.
How this unit is examined (End Sem pattern: any 5 of 6, 8 marks each)

1. Basic terms: phases in metal systems Medium

Definitions

Types of phases in alloys

Phase typeWhat it isExample
Substitutional solid solutionSolute atoms replace solvent atoms on lattice sitesCu–Ni (complete solubility), Cu–Zn (brass)
Interstitial solid solutionSmall solute atoms (C, N, H, B) sit in interstitial voidsC in γ-Fe (austenite), C in α-Fe (ferrite)
Intermediate phase / intermetallic compoundHas a fixed (or narrow) composition and its own crystal structure; usually hard and brittleFe₃C, CuAl₂ (θ), Mg₂Pb
Mechanical mixtureTwo or more phases intimately mixedPearlite (α + Fe₃C), eutectic Pb–Sn
Hume-Rothery rules (complete substitutional solubility)

(1) Atomic-size difference below about 15%. (2) Same crystal structure. (3) Similar electronegativity, otherwise intermetallics form. (4) Same valence; a metal dissolves a higher-valence metal more readily than a lower-valence one. Cu–Ni satisfies all four, so it is isomorphous.

2. Gibbs phase rule High Asked: End Sem 2024 (2 marks: derivation)

Formula

F = C − P + 2   (general)      F = C − P + 1   (condensed: pressure fixed at 1 atm)

F = degrees of freedom: the number of variables (T, P, composition) that can be changed independently without changing the number of phases. C = number of components. P = number of phases in equilibrium.

Model answer: derive the Gibbs phase rule (2 marks)

Consider a system of C components distributed among P phases in equilibrium.

  1. Total variables. The composition of each phase needs (C − 1) mole fractions, because the fractions add up to 1. For P phases that gives P(C − 1). Adding temperature and pressure: Variables = P(C − 1) + 2.
  2. Equations (constraints). At equilibrium, the chemical potential of each component is equal in every phase: μiα = μiβ = … gives (P − 1) equations per component. For C components: Equations = C(P − 1).
  3. Degrees of freedom = variables − equations = P(C − 1) + 2 − C(P − 1) = PC − P + 2 − PC + C, so F = C − P + 2.
  4. Metallurgical systems are studied at constant pressure (1 atm), which removes one variable, so F = C − P + 1 (condensed phase rule).
Worked examples (condensed rule, binary C = 2)
SituationPF = C − P + 1Meaning
Single-phase field (e.g. γ region)12T and composition can both vary (bivariant)
Two-phase field (e.g. α + L)21Fix T and the phase compositions are fixed by the tie-line (univariant)
Eutectic point, 1147 °C (L ⇌ γ + Fe₃C)30Invariant: T and all compositions fixed, so the cooling curve shows a plateau
Eutectoid point, 727 °C (γ ⇌ α + Fe₃C)30Invariant
Pure metal melting (C = 1, P = 2)21 − 2 + 1 = 0Melts at a fixed temperature
Triple point of water (general rule, C = 1, P = 3)31 − 3 + 2 = 0Unique T and P

3. Solidification of metals Medium

Solidification happens in two steps: nucleation (tiny stable solid particles form) and growth (those nuclei grow into grains). A liquid must be undercooled (ΔT = Tm − T) below the melting point before solid can form.

3.1 Homogeneous nucleation and the critical radius

Homogeneous nucleation happens uniformly inside the pure liquid, with no foreign surfaces. For a spherical embryo of radius r:

ΔG = (4/3)πr³ΔGv + 4πr²γ

ΔGv = free-energy change per unit volume. It is negative below Tm (the driving force) and grows with ΔT. γ = solid–liquid surface energy per unit area (always positive).

r* = −2γ / ΔGv     ΔG* = 16πγ³ / (3ΔGv²)

Using ΔGv = ΔHfΔT / Tm:   r* = −2γTm / (ΔHfΔT)

r*ΔG*+4πr²γ (surface)(4/3)πr³ΔGv (volume, ΔGv < 0)ΔG totalradius rFree energy ΔGembryo (r < r*) redissolvesnucleus grows
ΔG against embryo radius. Below r* the embryo redissolves; above r* the nucleus grows because adding atoms lowers ΔG. (Callister §10.3)
Worked numerical 1: critical radius

Q. For a metal, γ = 0.2 J/m² and ΔGv = −2 × 10⁸ J/m³. Find r* and ΔG*.

r* = −2γ/ΔGv = −2(0.2)/(−2 × 10⁸) = 2 × 10⁻⁹ m = 2 nm.

ΔG* = 16πγ³/(3ΔGv²) = 16π(0.008)/(3 × 4 × 10¹⁶) = 0.4021/(1.2 × 10¹⁷) = 3.35 × 10⁻¹⁸ J.

Worked numerical 2 (Callister Example 10.1, pure gold)

ΔHf = −1.16 × 10⁹ J/m³, γ = 0.132 J/m², Tm = 1064 °C = 1337 K, undercooling ΔT = 230 K.

r* = −2γTm/(ΔHfΔT) = −2(0.132)(1337)/[(−1.16 × 10⁹)(230)] = 352.97/(2.668 × 10¹¹) = 1.32 × 10⁻⁹ m = 1.32 nm.

ΔG* = 16πγ³Tm²/(3ΔHf²ΔT²) = ≈ 9.7 × 10⁻¹⁹ J (Callister gives 9.64 × 10⁻¹⁹ J). This nucleus is about 137 FCC unit cells, i.e. about 548 atoms.

3.2 Heterogeneous nucleation

3.3 Growth: planar and dendritic

3.4 Cast (ingot) structure

Chill zone — fine equiaxed (rapid cooling at mould wall)Columnar zone — elongated grains along heat flowCentral equiaxed zone — random nuclei, low ΔTMould wall (cross-section)
Three zones in a cast ingot.
  1. Chill zone: the liquid touching the cold mould wall cools very fast and nucleates heavily, giving a thin layer of fine, randomly oriented equiaxed grains.
  2. Columnar zone: grains with favourable orientation grow inward, opposite to the heat flow, as long column-like grains. This zone gives anisotropic properties.
  3. Central equiaxed zone: the remaining liquid has low undercooling. Broken dendrite arms and inoculants act as nuclei, giving coarse equiaxed grains. Shrinkage cavities (pipe) and segregation also gather here.

3.5 Cooling curves

Pure metalTm (plateau)Alloy (isomorphous)TLTSEutectic alloyTE (plateau)Ttime
A pure metal and a eutectic alloy both freeze at a constant temperature (F = 0, plateau). An isomorphous alloy freezes over a range from TL to TS (F = 1, change in slope).

4. Binary isomorphous system and solidification of alloys High

An isomorphous system has complete liquid and solid solubility, e.g. Cu–Ni (both FCC, Hume-Rothery rules satisfied). Its diagram has three regions: liquid, α (solid solution) and α + L, bounded by the liquidus (above it everything is liquid) and the solidus (below it everything is solid).

Three questions you can answer for any point (T, C₀):

  1. Phases present: read off the region the point lies in.
  2. Phase compositions: draw a horizontal tie-line across the two-phase field. Where it meets the liquidus gives CL; where it meets the solidus gives Cα.
  3. Phase amounts: use the lever rule.
CL=31.5C₀=35Cα=42.5BLiquidα (FCC solid solution)α + LLiquidusSolidus1100120013001400150012501085 (Cu)1455 (Ni)Composition (wt% Ni)T (°C)
Cu–Ni diagram with the tie-line at 1250 °C for a 35 wt% Ni alloy (point B). Data from Callister §9.8.
Lever rule (with derivation)

Mass balance: Wα + WL = 1  and  WαCα + WLCL = C₀. Solving these two equations:

WL = (Cα − C₀)/(Cα − CL)      Wα = (C₀ − CL)/(Cα − CL)

Memory trick: each phase's fraction = length of the opposite arm of the tie-line ÷ total tie-line length, with the fulcrum at C₀.

Worked numerical 3: Cu–Ni lever rule

Q. A 35 wt% Ni–Cu alloy is held at 1250 °C. Find the phases, their compositions and their amounts.

The point lies in the α + L field. Tie-line: CL = 31.5 wt% Ni, Cα = 42.5 wt% Ni.

WL = (42.5 − 35)/(42.5 − 31.5) = 7.5/11 = 0.68;   Wα = (35 − 31.5)/11 = 3.5/11 = 0.32.

Equilibrium and non-equilibrium solidification of an alloy

5. Invariant reactions: eutectic, eutectoid, peritectic, peritectoid High

E (61.9% Sn, 183 °C)Liquidαβα + Lβ + Lα + β18.397.80100183232327020406080100Composition (wt% Sn) Pb → SnT (°C)
Binary eutectic system (Pb–Sn), with limited solid solubility. α is Pb-rich and β is Sn-rich. Callister §9.11.

Key lines in a eutectic diagram: liquidus (two branches meeting at E), solidus, solvus (solubility limit of B in α and of A in β, decreasing as T falls) and the eutectic isotherm (183 °C).

Eutectic (Greek: "easily melted"): the composition with the lowest melting point. It freezes at one temperature into a lamellar mixture of α + β.

Alloys left of E are hypoeutectic (primary α + eutectic). Alloys right of E are hypereutectic (primary β + eutectic).

Soft solder (60Sn–40Pb) is close to the eutectic, so it melts sharply at a low temperature.

ReactionOn coolingExample (T, compositions)
EutecticL ⇌ α + β (one liquid gives two solids)Fe–C: L(4.30) → γ(2.14) + Fe₃C(6.70) at 1147 °C (ledeburite). Pb–Sn: L(61.9) → α(18.3) + β(97.8) at 183 °C
Eutectoidγ ⇌ α + β (one solid gives two solids)Fe–C: γ(0.76) → α(0.022) + Fe₃C(6.70) at 727 °C (pearlite). Cu–Zn: δ → γ + ε at 560 °C
PeritecticL + α ⇌ β (liquid + solid give a new solid)Fe–C: L(0.53) + δ(0.09) → γ(0.17) at 1493 °C. Cu–Zn: δ + L → ε at 598 °C
Peritectoidα + β ⇌ γ (two solids give a new solid)Rare; seen in a few systems (some Cu- and Ni-based alloys). Learn the form only.
MonotecticL₁ ⇌ L₂ + αCu–Pb (≈ 955 °C)
SyntecticL₁ + L₂ ⇌ αVery rare (e.g. Na–Zn)
Congruent transformationOne phase changes to another of the same compositionMelting of an intermetallic compound; pure-metal allotropy (α-Fe ⇌ γ-Fe at 912 °C)
Memory rule

"-ic" means a liquid is involved; "-oid" means everything is solid. Eu- means one phase splits into two on cooling; Peri- means two phases combine into one. All are invariant (F = 0, three phases in equilibrium) and show a horizontal line on the diagram.

6. The iron–iron carbide (Fe–Fe₃C) diagram High Asked: Mid Sem 2024 and End Sem 2024 (6 marks)

1538149313941147912727400Temperature (°C)00.762.144.306.70Composition (wt% C)Fe₃CSteelsCast ironsLiquid (L)γ + LγAusteniteγ + Fe₃Cα + Fe₃CL + Fe₃Cδ, δ+L, δ+γ (peritectic corner — see inset)α + γα (ferrite, BCC)A₃AcmA₁ (727 °C)Eutectic 4.30% C(Ledeburite)Eutectoid 0.76% C(Pearlite)0.0222.14Hypo-eutectoidHyper-eutectoid
Fe–Fe₃C phase diagram (metastable), after Callister Fig. 9.24. Orange lines are the critical lines used in heat treatment: A₁ (727 °C), A₃ (γ/α+γ) and Acm (γ/γ+Fe₃C). Steels: up to 2.14% C. Cast irons: 2.14–6.70% C.
0.090.170.53Lδδ + Lδ + γγ + Lγ (austenite)Peritectic line, 1493 °C15381493139400.20.40.6wt% C (magnified)
Peritectic (δ) corner, magnified.

Phases (learn all five)

PhaseStructure and max CProperties
α-ferriteBCC; 0.022% C at 727 °C (≈ 0.008% at room T)Soft, ductile, magnetic below 768 °C
γ-austeniteFCC; 2.14% C at 1147 °CSoft, ductile, non-magnetic; stable only above 727 °C in plain C steel
δ-ferriteBCC; 0.09% C at 1493 °CHigh-temperature form; little practical importance
Fe₃C (cementite)Orthorhombic; 6.70% CVery hard, brittle intermetallic; metastable (slowly turns into Fe + graphite)
Liquidabove the liquidus—

The three invariant reactions

ReactionTemperatureEquation (wt% C)Product
Peritectic1493 °CL (0.53) + δ (0.09) → γ (0.17)Austenite
Eutectic1147 °CL (4.30) → γ (2.14) + Fe₃C (6.70)Ledeburite (cast irons)
Eutectoid727 °Cγ (0.76) → α (0.022) + Fe₃C (6.70)Pearlite: alternating lamellae of α and Fe₃C (about 8 : 1 by mass)
Critical lines and other temperatures

Classification of iron–carbon alloys

Alloy% CRoom-temperature microstructure (slow cooling)
Commercially pure iron< 0.008Ferrite
Hypoeutectoid steel0.008–0.76Pro-eutectoid ferrite + pearlite
Eutectoid steel0.76100% pearlite
Hypereutectoid steel0.76–2.14Pearlite + pro-eutectoid cementite (network at the prior austenite grain boundaries)
Hypoeutectic white cast iron2.14–4.30Pearlite (from primary γ) + transformed ledeburite + Fe₃C
Eutectic cast iron4.30Transformed ledeburite (pearlite + Fe₃C)
Hypereutectic white cast iron4.30–6.70Primary Fe₃C needles + transformed ledeburite
Hypoeutectoid (e.g. 0.4% C)pro-eutectoid ferrite (white) + pearliteEutectoid (0.76% C)100% pearlite (α + Fe₃C lamellae)Hypereutectoid (e.g. 1.2% C)pearlite + grain-boundary Fe₃C network
Schematic room-temperature microstructures of slowly cooled steels.

Cooling of a 0.4% C (hypoeutectoid) steel

  1. Above about 800 °C (above A₃) the steel is fully austenite (γ).
  2. On crossing A₃ (≈ 800 °C), pro-eutectoid ferrite starts forming at the γ grain boundaries. The carbon it rejects enriches the remaining austenite.
  3. Between A₃ and 727 °C, the ferrite composition follows the α solvus and the austenite composition follows A₃ towards 0.76% C.
  4. At 727 °C the remaining austenite (now 0.76% C) undergoes the eutectoid reaction and becomes pearlite.
  5. At room temperature: pro-eutectoid ferrite (≈ 49%) + pearlite (≈ 51%).

Cooling of a 1.0% C (hypereutectoid) steel

  1. Above Acm (≈ 800 °C for 1.0% C) the steel is fully γ.
  2. Below Acm, pro-eutectoid cementite precipitates along the γ grain boundaries. The austenite loses carbon, moving down Acm towards 0.76%.
  3. At 727 °C the remaining γ (0.76% C) becomes pearlite.
  4. Final structure: pearlite + a grain-boundary cementite network. WFe₃C′ = (1.0 − 0.76)/(6.70 − 0.76) = 0.04, i.e. 4% pro-eutectoid cementite and 96% pearlite. The brittle network is removed by normalizing or spheroidizing.
Model answer: "Draw the Fe–C diagram, mark all phases and explain the reactions" (6 marks)

[Diagram, about 3 marks] Draw the figure above with axes T (°C) against wt% C (0 to 6.70). Mark 1538, 1493, 1394, 1147, 912 and 727 °C, and 0.022, 0.76, 2.14, 4.30 and 6.70% C. Label the fields L, δ, δ+L, δ+γ, γ, γ+L, L+Fe₃C, α, α+γ, γ+Fe₃C and α+Fe₃C, and the lines A₁, A₃ and Acm.

[Phases, 1 mark] α-ferrite (BCC, max 0.022% C); γ-austenite (FCC, max 2.14% C); δ-ferrite (BCC, max 0.09% C); cementite Fe₃C (6.70% C, hard and brittle); liquid.

[Reactions, 2 marks]

Each is invariant: by the condensed phase rule F = 2 − 3 + 1 = 0. Alloys up to 2.14% C are steels (hypo- and hypereutectoid on either side of 0.76%); 2.14–6.70% C are cast irons. Strong finish: one line each on the room-temperature structures of 0.4% C, 0.76% C and 1.2% C steel.

Lever-rule numericals on Fe–C High

Formulas just below 727 °C (Callister Eqs. 9.20–9.23)

Hypoeutectoid (C₀ < 0.76):   Wp = (C₀ − 0.022)/(0.76 − 0.022) = (C₀ − 0.022)/0.738    Wα′ = (0.76 − C₀)/0.738

Hypereutectoid (C₀ > 0.76):   Wp = (6.70 − C₀)/(6.70 − 0.76) = (6.70 − C₀)/5.94    WFe₃C′ = (C₀ − 0.76)/5.94

Total phases (any steel):   Wα = (6.70 − C₀)/(6.70 − 0.022) = (6.70 − C₀)/6.678    WFe₃C = (C₀ − 0.022)/6.678

Worked numerical 4: 0.40% C steel just below 727 °C

Pro-eutectoid ferrite: Wα′ = (0.76 − 0.40)/0.738 = 0.36/0.738 = 0.488 (48.8%)

Pearlite: Wp = (0.40 − 0.022)/0.738 = 0.378/0.738 = 0.512 (51.2%)

Total ferrite: Wα = (6.70 − 0.40)/6.678 = 6.30/6.678 = 0.943; total cementite WFe₃C = 0.057.

Eutectoid ferrite (the ferrite inside pearlite) = total α − pro-eutectoid α = 0.943 − 0.488 = 0.455.

Worked numerical 5: 0.25% C steel

Wα′ = (0.76 − 0.25)/0.738 = 0.51/0.738 = 0.691

Wp = (0.25 − 0.022)/0.738 = 0.228/0.738 = 0.309

Mostly ferrite, so the steel is soft and ductile. Low-carbon steels are used for sheet and wire.

Worked numerical 6: 1.2% C steel

WFe₃C′ = (1.2 − 0.76)/5.94 = 0.44/5.94 = 0.074

Wp = (6.70 − 1.2)/5.94 = 5.50/5.94 = 0.926

Total α = 5.50/6.678 = 0.824; total Fe₃C = 0.176.

Worked numerical 7: eutectoid steel

Ferrite and cementite in pearlite (0.76% C):

Wα = (6.70 − 0.76)/(6.70 − 0.022) = 5.94/6.678 = 0.889; WFe₃C = 0.111, i.e. about 8 : 1. That is why the ferrite lamellae are much thicker than the cementite lamellae.

Worked numerical 8: reverse problem

Q. A slowly cooled plain carbon steel shows 60% pearlite and 40% pro-eutectoid ferrite. Find its carbon content.

Wp = (C₀ − 0.022)/0.738 = 0.60, so C₀ = 0.022 + 0.443 = 0.465 ≈ 0.46% C.

7. TTT (isothermal transformation) diagram High Asked: End Sem 2024 (4 marks)

A₁ = 727 °C (eutectoid)Austenite (stable)Ms ≈ 220 °CM50M90 (Mf approached)Austenite → Martensite (diffusionless)Coarse pearliteFine pearliteBainite(upper above ~350, lower below)Unstableaustenitenose ≈ 540 °C, ~1 sCritical cooling rate10-1110102103104105Time (s, log scale)0200400600800Temperature (°C)
TTT diagram for eutectoid (0.76% C) steel, after Callister Fig. 10.23. Solid C-curve = start of transformation (1%); dashed curve = finish (99%). The dotted orange line is the critical cooling rate, just missing the nose. (Cooling curves strictly belong on a CCT diagram; examiners accept them on a TTT sketch.)

Construction

  1. Prepare many small samples of eutectoid steel and austenitize them (above 727 °C, fully γ).
  2. Quench each into a salt bath at a fixed sub-critical temperature (e.g. 700, 650, 600 … °C) and hold isothermally.
  3. Remove samples after increasing times and quench them in water. Untransformed austenite becomes martensite, so the microscope shows how much austenite had already transformed.
  4. Plot the times for 1% (start) and 99% (finish) transformation at each temperature on a log-time axis. The points form "C"-shaped curves (S-curves).

Why the C-shape?

Just below A₁ the undercooling is small, so the driving force (nucleation) is low and transformation is slow. At low temperature, diffusion is slow. At the nose (≈ 540 °C, under 1 s) the balance of driving force and diffusion gives the fastest transformation.

Regions and products

Transformation temperatureProductStructureHardness (approx.)
727–650 °CCoarse pearliteThick α + Fe₃C lamellae (high T, fast diffusion)≈ HRC 15–20
650–540 °CFine pearliteThin lamellae≈ HRC 30–40
540–350 °CUpper bainiteFeathery: ferrite laths with Fe₃C between them≈ HRC 40–45
350 °C to MsLower bainiteAcicular (needle-like): ferrite plates with fine carbides inside≈ HRC 50–60
Below Ms (≈ 220 °C)MartensiteBCT supersaturated solid solution, needle/lath-like; diffusionless shearup to HRC 65

Effect of carbon and alloying elements

TTT vs CCT

TTT (isothermal transformation)CCT (continuous cooling transformation)
Transformation at constant temperatureTransformation during continuous cooling (real heat treatment)
Used for austempering, martempering and isothermal annealingUsed for annealing, normalizing and quenching
C-curves further left and higherCurves shifted down and to the right (longer times, lower temperatures)
Bainite region presentBainite usually absent for plain-carbon eutectoid steel; the cooling path cuts off at the pearlite "nose"
Model answer: "Draw the TTT diagram for eutectoid steel, label regions and products" (4 marks)
  1. Draw: temperature (0–800 °C) against log time (0.1 to 10⁵ s). Draw the A₁ line at 727 °C, the start (1%) and finish (99%) C-curves with the nose at ≈ 540 °C and ≈ 1 s, and horizontal lines Ms ≈ 220 °C, M50 and M90.
  2. Label the regions: stable austenite above A₁; unstable austenite left of the start curve; austenite + product between the curves; the transformed product right of the finish curve.
  3. Products: coarse pearlite (727–650 °C), fine pearlite (650–540 °C), upper bainite (540–350 °C), lower bainite (350 °C to Ms), martensite below Ms (diffusionless).
  4. Add one line on the critical cooling rate (tangent to the nose, gives 100% martensite) and one on the C-shape (nucleation vs diffusion).
PearliteBainiteMartensite
Forms at727–540 °C540 °C – Msbelow Ms
MechanismDiffusion (nucleation and growth)Diffusion of C + shear of FeDiffusionless shear (athermal)
Phasesα + Fe₃C lamellaeα + fine Fe₃C (non-lamellar)Single phase, BCT, C supersaturated
PropertiesSoft–moderate, ductileStrong and toughHardest, brittle; must be tempered

8. Heat treatment of plain carbon steels High

Heat treatment means heating a metal in the solid state to a set temperature, holding it (soaking) and cooling it at a controlled rate to get the microstructure and properties you want.

Normalizing(+55–85 °C above A₃/Acm)Full annealing & hardening(+15–40 °C)SpheroidizingProcessannealingTempering: 150–650 °C (below A₁)A₃AcmA₁ 727600727800912100000.40.761.21.6wt% C (steel corner of Fe–Fe₃C)Temperature (°C)
Heat-treatment temperature ranges on the steel corner of the Fe–Fe₃C diagram (after Callister Fig. 11.10).

8.1 Annealing Asked: End Sem 2024 (with normalizing, 3 marks)

TypeTemperatureCoolingResult and purpose
Full annealing15–40 °C above A₃ (hypo) or above A₁ (hyper)Very slow, in the furnaceCoarse pearlite (+ ferrite or cementite). Softest condition; best ductility and machinability for low/medium-C steel; refines a coarse cast structure; relieves stresses
Process (sub-critical) annealingBelow A₁, about 550–650 °CAirRecovery and recrystallization of cold-worked low-C sheet or wire, so it can be worked further; no phase change
SpheroidizingJust below A₁ (≈ 700 °C) for 15–25 h, or cycling about A₁SlowFe₃C becomes spheres in a ferrite matrix (spheroidite): softest, most ductile structure; best machinability for high-C (tool) steels
Stress-relief annealingAbout 550–650 °C (below A₁)SlowRemoves residual stresses from welding, machining, casting or cold work; no change in microstructure

Why hypereutectoid steels are not heated above Acm for annealing: on slow cooling a continuous brittle Fe₃C network would form at the grain boundaries.

8.2 Normalizing

Model answer: "Discuss annealing and normalizing in terms of their effects on microstructure" (3 marks)
Full annealingNormalizing
Heating15–40 °C above A₃ (hypo) / A₁ (hyper)55–85 °C above A₃ / Acm
CoolingFurnace (very slow)Still air (faster)
MicrostructureCoarse pearlite + pro-eutectoid phase; larger grainsFine pearlite; finer, more uniform grains; cementite network broken up
PropertiesSofter, more ductile, lower strengthHigher hardness, strength and toughness
Cost/timeLonger, costlier (furnace occupied)Shorter, cheaper

Reason: faster air cooling means more undercooling, so austenite transforms at a lower temperature. Diffusion distances are shorter (thinner lamellae) and nucleation is more frequent (finer grains).

8.3 Hardening

8.4 Tempering

Reheat hardened steel below A₁ (150–650 °C), hold, then cool. This relieves quenching stresses and trades a little hardness for toughness and ductility. The product is tempered martensite: fine Fe₃C particles in a ferrite matrix.

StageTemperatureChange
180–200 °Cε-carbide (Fe₂.₄C) precipitates; martensite loses some tetragonality; stresses are relieved (low-temperature tempering for tools: hardness kept)
2200–300 °CRetained austenite decomposes to bainite-like ferrite + carbide
3250–400 °Cε-carbide becomes cementite; martensite becomes ferrite + fine Fe₃C (troostite); medium-temperature tempering for springs
4400–650 °CFe₃C coarsens and spheroidizes (sorbite); recovery of ferrite; high toughness for shafts, axles and gears
Temper embrittlement

8.5 Martempering and austempering (isothermal treatments)

Martempering (marquenching)

Quench into a salt bath just above Ms. Hold only until the temperature is uniform through the section (before bainite starts). Then air-cool through the Ms–Mf range, giving martensite, then temper.

Benefit: the surface and core turn to martensite together, so there is much less distortion, residual stress and cracking.

Austempering

Quench into a salt bath above Ms (≈ 260–400 °C) and hold until transformation to bainite is complete, then air-cool.

Benefit: lower bainite has better toughness and ductility than tempered martensite at the same hardness, less distortion, and no tempering is needed. Limited to thin sections.

8.6 Hardenability and the Jominy end-quench test High

Definition

Hardenability is a steel's ability to form martensite to a certain depth when quenched. It is different from hardness, which is resistance to indentation; the maximum hardness depends mainly on % C. A high-hardenability steel hardens all the way to the core.

FixtureWater jet100 mmØ 25 mmquenched endAlloy steel (e.g. 4340): high hardenabilityPlain carbon (1040): low hardenabilityDistance from quenched end →Hardness (HRC)
Jominy end-quench test: setup and hardness profile.
  1. Specimen: a standard bar 25 mm (1 in.) in diameter and 100 mm (4 in.) long.
  2. Austenitize it at the specified temperature for a specified time.
  3. Mount it in a fixture and quench only the bottom end with a water jet of specified flow and temperature. The cooling rate is highest at the quenched end and falls along the length.
  4. After cooling, grind a flat 0.4 mm deep along the length and measure Rockwell C hardness every 1.6 mm (1/16 in.) for the first 50 mm.
  5. Plot the hardenability curve (hardness against distance from the quenched end). A flatter curve means higher hardenability.

Factors that increase hardenability: alloying elements (Cr, Mo, Ni, Mn, B), which shift the TTT curve right; higher carbon (up to eutectoid); coarser austenite grain size; homogeneous austenite. Severity of quench and section size decide the actual cooling rate.

8.7 Surface (case) hardening High

Aim: a hard, wear-resistant surface (case) on a tough, ductile core, for gears, cams, camshafts and piston pins. There are two ways:

ProcessMedium and temperatureElement addedCase depthQuench?Notes
Pack carburizingBox with charcoal + energizer (BaCO₃/Na₂CO₃), 900–950 °C, several hoursC (surface ≈ 0.8–1% C)0.5–2 mmYes, then temperLow-C steels (0.1–0.2% C); simple, but slow and hard to control
Gas carburizingCH₄/propane + carrier gas, 870–950 °CC0.1–1.5 mmYes (direct)Accurate control, clean, mass production
Liquid carburizingMolten cyanide-based salt bath, 815–900 °CC (+ a little N)0.1–0.8 mmYesFast, uniform heating; toxic salts
CyanidingMolten NaCN bath, 800–870 °C, 30–60 minC + N0.1–0.3 mmYes (direct water/oil)Thin, hard case on small parts (screws, small gears); highly poisonous
CarbonitridingCarburizing gas + NH₃, 750–900 °CC + N0.07–0.75 mmYes (oil)Gas version of cyaniding; less distortion than carburizing
NitridingNH₃ gas, 500–590 °C (below A₁), 10–100 hN, forming hard nitrides with Al, Cr, Mo (Nitralloy)0.1–0.6 mmNoHardest case (≈ 1000–1100 HV), minimal distortion, good fatigue and corrosion resistance; done after hardening and tempering; slow, costly

Induction hardening

A copper coil carries high-frequency AC around the part. Induced eddy currents heat a thin surface layer above A₃ within seconds, and a water spray quenches it to martensite. The skin effect means a higher frequency gives a shallower case. Used for medium-C steels (0.35–0.6% C): crankshafts, camshafts, gear teeth, axles.

Flame hardening

An oxy-acetylene flame heats the surface above the upper critical temperature, followed immediately by a water spray. Used for large or irregular parts that won't fit a furnace (lathe beds, large gears, rolls). Case depth depends on flame speed, intensity and dwell time.

Induction hardeningFlame hardening
Eddy-current heating; very fast (seconds)Oxy-fuel flame; slower
Case depth precisely controlled by frequency and power (≈ 0.5–5 mm)Less control; deeper cases (≈ 1.5–6 mm)
High equipment cost; ideal for mass production, easily automatedCheap, portable; suits one-off and very large parts
Little scaling, decarburization or distortionRisk of overheating, uneven hardness, some scaling
Exam tip: carburizing vs nitriding (a favourite 3–4 mark comparison)

Carburizing: C, 900–950 °C (in the austenite range), quench needed, more distortion, case ≈ 60 HRC, cheaper, faster. Nitriding: N, 500–590 °C (ferrite range), no quench, minimal distortion, harder case (≈ 70 HRC), needs alloying elements (Al, Cr, Mo), slow (up to 100 h).

9. Precipitation (age) hardening of aluminium alloys High

Precipitation hardening strengthens an alloy with extremely small, uniformly dispersed second-phase particles that block dislocation motion. It is the main strengthening method for Al alloys, which can't be hardened by martensite. (Callister §11.10)

Requirements

(1) The maximum solubility of the solute must be fairly high. (2) The solubility must fall sharply as temperature drops. Al–Cu: maximum Cu solubility in α-Al is about 5.65% at 548 °C, dropping to nearly zero at room temperature. Al–4% Cu (duralumin-type 2014/2024 alloys) qualifies.

Solution treat ~540 °C (α only)Quench(SSSS)Age 150–190 °C(or room temp:natural aging)timeTT₁ (higher)T₂ < T₁: higher peak, laterGP zones → θ″peak: θ″ + θ′overaged: coarse θAging time (log) →Hardness / strength
Left: precipitation-hardening heat-treatment cycle. Right: hardness against aging time at two temperatures (T₂ < T₁).
  1. Solution heat treatment: heat Al–4% Cu to about 500–548 °C (into the single-phase α field, between solvus and solidus) and hold until all the θ (CuAl₂) dissolves.
  2. Quenching: cool rapidly to room temperature (water). There is no time for θ to form, so you get a supersaturated solid solution (SSSS) of Cu in Al. It is soft and ductile, so it can be formed now (e.g. rivets).
  3. Aging: natural aging at room temperature, or artificial aging at 100–200 °C. Precipitation proceeds in this sequence:

    SSSS → GP zones (GP-I) → θ″ (GP-II) → θ′ → θ (CuAl₂)

    • GP zones: Cu-rich discs one or two atoms thick, fully coherent with the matrix.
    • θ″: coherent, tetragonal; produces large coherency strains. θ′: semi-coherent.
    • Peak hardness occurs when θ″/θ′ are present: coherency strain fields strongly resist dislocations.
    • Overaging: longer time or higher temperature gives coarse, incoherent equilibrium θ. The particles are farther apart and dislocations bypass them, so strength falls.

Quick revision: numbers to memorize High

ItemValueItemValue
Fe melting1538 °CEutectic1147 °C, 4.30% C
δ → γ (pure Fe)1394 °CMax C in γ2.14% at 1147 °C
γ → α (pure Fe)912 °CEutectoid727 °C, 0.76% C
Curie point (A₂)768 °CMax C in α0.022% at 727 °C
Peritectic1493 °C; 0.09 / 0.17 / 0.53% CFe₃C6.70% C
Nose of TTT (eutectoid)≈ 540 °C, ≈ 1 sMs (eutectoid steel)≈ 220 °C
Nitriding500–590 °C, NH₃, no quenchCarburizing900–950 °C
Tempering range150–650 °CAl–Cu solution treatment≈ 500–548 °C, age 100–200 °C

Likely exam questions

The typical DTU pattern, built from the topics above. These are practice questions, not reproduced past papers. Marks shown match the 8-mark question format (6+2, 5+3, 4+4).

  1. Draw the Fe–Fe₃C equilibrium diagram, label all phases and temperatures, and write the invariant reactions. (6)
  2. Derive the Gibbs phase rule. Apply it to the eutectoid point of the Fe–C system. (2–3)
  3. Draw the TTT diagram for eutectoid steel and label the regions and products. What is the critical cooling rate? (4–5)
  4. Discuss annealing and normalizing in terms of their effects on microstructure and properties. (3–4)
  5. Calculate the amounts of pro-eutectoid ferrite, pearlite, total ferrite and total cementite in a 0.4% C steel just below 727 °C. (3–4)
  6. State and derive the lever rule. For a 35 wt% Ni–Cu alloy at 1250 °C (CL = 31.5, Cα = 42.5), find the phase fractions. (4)
  7. Explain eutectic, eutectoid, peritectic and peritectoid reactions with one example of each. (4)
  8. Differentiate homogeneous and heterogeneous nucleation. Derive the expression for the critical radius of a nucleus. (5)
  9. What is hardenability? Describe the Jominy end-quench test with a sketch. (4)
  10. Explain carburizing and nitriding, and compare them. (4)
  11. Write short notes on (a) induction hardening, (b) flame hardening, (c) cyaniding. (2 each)
  12. Explain the stages of tempering. What is temper embrittlement? (4)
  13. Explain precipitation hardening of Al–4% Cu alloy with a neat sketch. What is overaging? (5)
  14. Differentiate martempering and austempering. Compare pearlite, bainite and martensite. (4)
Model answer: homogeneous vs heterogeneous nucleation, and the r* derivation (5 marks)

Difference (2 marks): Homogeneous nucleation happens uniformly throughout the pure liquid without help from foreign surfaces, and needs large undercooling (≈ 0.2Tm). Heterogeneous nucleation happens on mould walls, impurities or inoculants. The surface lowers the barrier (ΔG*het = S(θ)ΔG*hom), so only a few degrees of undercooling are needed. All practical castings nucleate this way.

Derivation (3 marks): ΔG = (4/3)πr³ΔGv + 4πr²γ (with ΔGv < 0). At the maximum, dΔG/dr = 4πr²ΔGv + 8πrγ = 0, so r* = −2γ/ΔGv. Substituting back: ΔG* = 16πγ³/(3ΔGv²). Since ΔGv = ΔHfΔT/Tm, r* = −2γTm/(ΔHfΔT): more undercooling means a smaller r*, more nuclei and finer grains. Sketch the ΔG–r curve.

Model answer: carburizing vs nitriding (4 marks)
CarburizingNitriding
Element diffusedCarbonNitrogen
Temperature900–950 °C (austenite)500–590 °C (ferrite, below A₁)
MediumCharcoal + BaCO₃ (pack), CH₄ (gas), cyanide salts (liquid)Dissociated ammonia: 2NH₃ → 2N + 3H₂
SteelLow-C (0.1–0.2%) plain or alloyAlloy steels with Al, Cr, Mo (Nitralloy)
Post-treatmentQuench + temper requiredNo quench; done on hardened and tempered parts
Case hardness / depth≈ 60 HRC; 0.5–2 mm≈ 1000–1100 HV; 0.1–0.6 mm
Distortion, timeMore distortion; a few hoursMinimal distortion; 10–100 h
Model answer: precipitation hardening of Al–4% Cu (5 marks)

Draw the Al-rich corner of the Al–Cu diagram (solvus rising to 5.65% Cu at 548 °C) or the thermal cycle, plus the aging curve. Then three steps: (1) solution treatment at about 540 °C, giving single-phase α; (2) quench, giving a soft supersaturated α (SSSS); (3) aging at room temperature or 100–200 °C, with precipitation sequence GP zones → θ″ → θ′ → θ (CuAl₂). Coherent θ″/θ′ particles create strain fields that block dislocations, giving peak hardness. Prolonged aging gives coarse incoherent θ and overaging (softening). A lower aging temperature gives a higher peak after a longer time. Used in aircraft alloys 2014/2024.

Unit 4 · ~6 contact hrs

Fracture, Fatigue & Creep

Most examined: Griffith derivation (6 marks), KIc / surface-energy numericals (2–3 marks), creep curve with mechanisms, DBTT, S–N curve.

1. Elastic behaviour: Hooke's law, E, G, ν Medium

Definition

Elastic deformation is non-permanent: the material returns to its original shape when the load is removed. Inside the elastic region stress is proportional to strain (Hooke's law): σ = Eε. The constant E (modulus of elasticity, Young's modulus) measures stiffness, i.e. resistance to elastic deformation. Atomically, E is the slope of the interatomic force–separation curve at the equilibrium spacing, so it depends on bond strength.

Formulas
σ = F/A₀    ε = Δl/l₀    σ = Eε    τ = Gγ
ν = −εlateral/εaxial = −εx/εz    E = 2G(1 + ν)

For most metals ν ≈ 0.25–0.35, so G ≈ 0.4E. E falls slowly as temperature rises.

MaterialE (GPa)G (GPa)ν
Steel207830.30
Copper110460.34
Aluminium69250.33
Tungsten4071600.28
Ceramics (Al₂O₃)380—0.22
Polymers0.007–4—~0.4
Worked numerical

A copper bar (E = 110 GPa), originally 305 mm long, is pulled in tension with a stress of 276 MPa. The deformation is entirely elastic. Find the elongation.

Δl = σl₀/E = (276 × 10⁶ × 305)/(110 × 10⁹) = 0.77 mm.

Steel has E = 207 GPa and ν = 0.30, so G = E/[2(1 + ν)] = 207/2.6 = 79.6 GPa.

2. Yield point, strength & the stress–strain curve High

Upper YP Lower YP(Lüders band) UTS necking fracture elastic Strain ε Stress σ (a) Low-C steel: distinct yield σy at the 0.2 % offset a brittle material fractures here, with no plastic region 0.002 Strain ε (b) No distinct yield: 0.2 % offset
Engineering stress–strain curves. Area under the elastic part is the resilience; area under the whole curve is the toughness.

Key points on the curve

True stress and true strain (valid up to necking)
σT = F/Ai = σ(1 + ε)     εT = ln(li/l₀) = ln(1 + ε)     σT = KεTn

n is the strain-hardening exponent. True stress keeps rising after the UTS because the actual area keeps shrinking.

Worked numerical

At an engineering stress of 400 MPa the engineering strain is 0.20. Then σT = 400(1.20) = 480 MPa and εT = ln 1.20 = 0.182.

Resilience of a steel with σy = 300 MPa and E = 207 GPa: Ur = (300 × 10⁶)²/(2 × 207 × 10⁹) = 2.17 × 10⁵ J/m³.

3. Fracture in ductile and brittle materials High

Definition

Fracture is the separation of a body into two or more pieces under a static stress, at temperatures that are low relative to Tm. It has two steps: crack formation and crack propagation. Ductile fracture involves extensive plastic deformation and a slow, stable crack that resists extension. Brittle fracture involves little or no plastic deformation and a fast, unstable crack that runs once it starts.

Ductile fracture: the cup-and-cone sequence

(a) Necking (b) Microvoids format inclusions (c) Voids coalesceinto a crack (d) Crack grows⟂ to the load (e) Shear at 45°:cup and cone
Stages of cup-and-cone fracture (Callister §8.3). The fibrous central region is surrounded by a 45° shear lip, where shear stress is maximum.

Under the SEM, a ductile fracture surface shows dimples: half-voids, spherical under uniaxial tension and parabolic under shear.

Brittle fracture

FeatureDuctile fractureBrittle fracture
Plastic deformationExtensive (necking)Little or none
Crack growthSlow and stable; needs increasing stressVery fast and unstable; self-propagating
Energy absorbedHigh (tough)Low
Warning before failureYes (visible deformation)No (catastrophic)
Fracture surfaceCup and cone, fibrous, dull, dimplesFlat, granular or shiny, chevron marks
Fracture plane45° shear lip plus central fibrous zone⟂ to the tensile axis
ExamplesMild steel, Cu, Al, Au at room temperatureCast iron, glass, ceramics, steel below its DBTT

4. Griffith's theory of brittle fracture High Asked: End Sem 2024 (6 marks)

Why real strength is far below theoretical strength

The theoretical cohesive strength of a solid is about E/10. Measured fracture strengths of brittle materials are 10 to 1000 times lower. Griffith (1920) explained this by the presence of very small microscopic flaws or cracks, always present at the surface and inside a body, which act as stress raisers.

2a tip radius ρt σ₀σ₀ σm = 2σ₀√(a/ρt) σ₀ crack crack tip distance x local stress σ
An elliptical crack of length 2a in a plate under remote stress σ₀. The local stress peaks at the crack tip.
Stress concentration at a crack tip (Inglis)
σm = 2σ₀ (a/ρt)1/2      Kt = σm/σ₀ = 2(a/ρt)1/2

Here a is the length of a surface crack, or half the length of an internal crack. Long, sharp cracks (large a, small ρt) give the largest concentration. In ductile metals, plastic flow at the tip blunts the crack, so Kt is smaller.

Model answer: Griffith energy-balance derivation (6 marks)

Assumptions. The material is ideally brittle and linear elastic. It is a thin infinite plate of unit thickness under plane stress. It contains a through-thickness elliptical crack of length 2a, normal to a uniform tensile stress σ.

Statement. A crack propagates when the elastic strain energy released by its growth is equal to, or greater than, the energy needed to create the new crack surfaces.

Step 1: strain energy released. Introducing the crack relaxes the stress in a region around it. For unit thickness, the stored elastic energy falls by

UE = −πa²σ²/E

Step 2: surface energy gained. The crack has two faces, each 2a long (unit thickness), so the new surface area is 4a. With γs the specific surface energy (J/m²):

US = 4aγs

Step 3: total energy change.

ΔU = 4aγs − πa²σ²/E

ΔU first rises with a (surface term dominates) and then falls (strain-energy term dominates). The crack becomes unstable at the maximum of ΔU.

Step 4: condition for propagation. Set d(ΔU)/da = 0:

4γs − 2πaσ²/E = 0  ⇒  σ² = 2Eγs/(πa)

σc = (2Eγs / πa)1/2

Conclusions.

Draw: (i) the plate with the crack and the stress arrows, and (ii) the ΔU vs a curve with its maximum at the critical crack length ac.

surface energy +4aγs strain energy −πa²σ²/E ΔU total (maximum at a = ac) ac a ΔU
Energy versus crack length. Beyond ac, crack growth lowers the total energy, so the crack runs unstably.
Worked numerical 1: Griffith critical flaw size (Callister Ex. 8.1)

A relatively large glass plate is loaded in tension at 40 MPa. Surface energy γs = 0.3 J/m² and E = 69 GPa. Find the maximum length of surface flaw possible without fracture.

ac = 2Eγs/(πσ²) = (2 × 69 × 10⁹ × 0.3)/(π × (40 × 10⁶)²) = (4.14 × 10¹⁰)/(5.027 × 10¹⁵) = 8.2 × 10⁻⁶ m = 8.2 µm.

Worked numerical 2: surface energy from KIc (End Sem 2024 type, 2 marks)

A material has fracture toughness 80 MPa√m and critical crack length 0.05 mm, with E = 120 GPa. Calculate the surface energy γ.

Griffith gives σc²πa = 2Eγ. Since KIc = σc√(πa), we get KIc² = 2Eγ, so

γ = KIc²/(2E) = (80 × 10⁶)²/(2 × 120 × 10⁹) = 6.4 × 10¹⁵/2.4 × 10¹¹ = 2.67 × 10⁴ J/m².

The crack length cancels out; it is needed only if you are also asked for σc. Here σc = KIc/√(πa) = 80/√(π × 5 × 10⁻⁵) = 80/0.01253 = 6.38 × 10³ MPa. A value of 2.67 × 10⁴ J/m² is far larger than a true surface energy (~1 J/m²). It is really (γs + γp), dominated by plastic work at the crack tip (Orowan). Write this line; it earns the remaining mark.

Worked numerical 3: Griffith fracture stress

A glass (E = 70 GPa, γs = 1.0 J/m²) contains an internal crack 4 µm long (a = 2 µm). Find the fracture stress.

σc = √(2Eγs/πa) = √(2 × 70 × 10⁹ × 1.0/(π × 2 × 10⁻⁶)) = √(2.228 × 10¹⁶) = 1.49 × 10⁸ Pa ≈ 149 MPa.

Compared with the theoretical strength E/10 = 7 GPa, the flaw lowers the strength about 47 times.

Worked numerical 4: stress concentration

A surface crack is 0.5 mm deep with tip radius 5 × 10⁻³ mm. The applied stress is 100 MPa.

σm = 2σ₀√(a/ρt) = 2 × 100 × √(0.5/0.005) = 2 × 100 × 10 = 2000 MPa, so Kt = 20.

Worked numerical 5: critical crack length from E and γ

For a brittle ceramic, E = 300 GPa and γs = 0.8 J/m². What internal crack length 2a causes fracture at 200 MPa?

a = 2Eγs/(πσ²) = (2 × 300 × 10⁹ × 0.8)/(π × 4 × 10¹⁶) = 4.8 × 10¹¹/1.257 × 10¹⁷ = 3.82 × 10⁻⁶ m, so the crack length 2a = 7.6 µm.

5. Fracture toughness KIc High

Definition

The stress intensity factor K describes the stress field near a crack tip. Fracture toughness Kc is the critical value of K at which a crack propagates rapidly. It measures a material's resistance to brittle fracture when a crack is present. Units: MPa√m.

Formulas
Kc = Yσc√(πa)     σc = KIc/(Y√(πa))     ac = (1/π)[KIc/(Yσ)]²
Plane-strain condition: B ≥ 2.5 (KIc/σy)²

Y is a dimensionless geometry factor (≈ 1 for a centre crack in a wide plate; ≈ 1.1 for an edge crack). B is the specimen thickness.

Modes of crack-surface displacement

Mode I: openingtensile stress ⟂ crack Mode II: sliding (in-plane shear)shear ∥ crack growth direction Mode III: tearing (anti-plane)out of pageinto pageshear ∥ crack front
Mode I (opening) is the most common in practice and the most severe. Hence the subscript "I" in KIc.
Materialσy (MPa)KIc (MPa√m)
Al alloy 7075-T65149524
Ti-6Al-4V91055
4340 steel (tempered 260 °C)164050
4340 steel (tempered 425 °C)142087.4
Soda-lime glass—0.7–0.8
Al₂O₃—2.7–5.0
Concrete—0.2–1.4

Callister Table 8.1. Note the trade-off: the 4340 steel with higher σy has lower KIc.

Worked numerical 6: KIc design

A steel plate has KIc = 50 MPa√m and Y = 1.1 (edge crack). (a) Find the critical crack length at a design stress of 250 MPa. (b) If NDT can detect cracks only down to 3 mm, what is the safe design stress?

(a) ac = (1/π)(KIc/Yσ)² = (1/π)(50/275)² = (1/π)(0.03306) = 0.0105 m ≈ 10.5 mm.

(b) σc = KIc/(Y√(πa)) = 50/(1.1 × √(π × 0.003)) = 50/(1.1 × 0.0971) = 468 MPa. Cracks smaller than 3 mm cannot be detected, so the plate must be designed for σ < 468 MPa, with a factor of safety on top.

Worked numerical 7: is plane strain valid?

For 4340 steel tempered at 260 °C (σy = 1640 MPa, KIc = 50 MPa√m): B ≥ 2.5(50/1640)² = 2.5 × 9.30 × 10⁻⁴ = 2.3 × 10⁻³ m. A plate thicker than 2.3 mm is in plane strain.

6. Ductile-to-brittle transition (DBTT) High

Impact tests (Charpy and Izod) measure the energy absorbed in breaking a notched bar struck by a swinging pendulum. The energy equals the drop in pendulum height × weight. In the Charpy test the specimen (10 × 10 × 55 mm, 2 mm V-notch) is simply supported as a beam and struck behind the notch. In the Izod test it is clamped vertically as a cantilever and struck above the notch. Severe conditions (notch, high strain rate, low temperature) bring out any tendency to brittle behaviour.

FCC metals (Al, Cu, austenitic SS): no transition BCC metals, low-carbon steel brittle (lower shelf) ductile (upper shelf) DBTT Temperature Impact energy (J)
Impact energy versus temperature. The fracture surface changes from fibrous (shear) to granular (cleavage) as temperature falls (Callister §8.6).

7. Fatigue High

Definition

Fatigue is failure under fluctuating (cyclic) stresses at a stress level much lower than the tensile or yield strength, after a long period of service. It causes about 90 % of metallic failures, for example in shafts, bridges, aircraft and springs. It is brittle-like (little gross deformation) and catastrophic.

(a) Reversed: σm = 0, R = −1tσ σmaxσmσmin σaσr (b) Repeated: σm ≠ 0t (c) Random stress cycle
Types of fatigue stress cycle.
Cyclic stress parameters
σm = (σmax + σmin)/2    σr = σmax − σmin    σa = σr/2 = (σmax − σmin)/2    R = σmin/σmax

Tensile stresses are positive and compressive negative. Fully reversed loading: R = −1. Zero-to-tension: R = 0.

Worked numerical 8

σmax = 400 MPa, σmin = −100 MPa. Then σm = (400 − 100)/2 = 150 MPa, σr = 500 MPa, σa = 250 MPa and R = −100/400 = −0.25.

Reverse problem: given σm = 70 MPa and σa = 210 MPa, σmax = 70 + 210 = 280 MPa, σmin = 70 − 210 = −140 MPa and R = −0.5.

S–N curve (Wöhler curve)

Steel, Ti alloys: endurance limit Al, Cu, Mg alloys: no limit fatigue limit Se fatigue strength at 10⁷ 10³10⁴10⁵10⁶10⁷10⁸10⁹ Cycles to failure N (log) Stress amplitude S
S–N curves: ferrous materials (typical) versus non-ferrous materials (Callister §8.8).

Crack initiation and propagation

  1. Crack initiation: a small crack forms at a point of high stress concentration on the surface: scratches, sharp fillets, keyways, threads, dents, or persistent slip bands (intrusions and extrusions).
  2. Crack propagation: the crack advances by a small increment with each cycle. Stage I is slow, along slip planes. Stage II is faster, ⟂ to the stress.
  3. Final failure: very rapid, once the crack reaches its critical size, i.e. when K reaches Kc in the reduced section.

Beach marks (clamshell marks) are macroscopic, visible to the eye, concentric ridges. They form when loading is interrupted, and they mark the crack front positions. Striations are microscopic (SEM). Each striation is the crack advance in one cycle, and one beach mark contains thousands of striations. The final fast-fracture zone is rough and granular.

origin beach marks spread from origin top: final rapid fracture
Fatigue fracture surface of a shaft.
Crack growth rate (Paris law)
da/dN = A(ΔK)m,   ΔK = Yσr√(πa)    (m ≈ 1–6)

Integrating from the initial crack size a₀ to the critical size ac gives the fatigue life Nf.

Factors affecting fatigue life and design considerations

FactorEffect and remedy
Mean stressHigher σm shortens life at the same σa.
Design: stress raisersAvoid sharp corners, holes, keyways and abrupt changes in section. Use generous fillet radii.
Surface finishPolishing removes machining scratches and raises life.
Residual surface stressShot peening (small hard shot, 0.1–1 mm, blasted onto the surface) puts a thin layer in compressive residual stress, which offsets the tensile cycle and slows crack initiation.
Case hardeningCarburizing or nitriding gives a hard, wear-resistant case in compressive residual stress, so the fatigue life rises.
DecarburizationA soft surface lowers fatigue life, so avoid it.
EnvironmentThermal fatigue: cycles of thermal stress σ = αEΔT. Reduce restraint and temperature gradients. Corrosion fatigue: corrosion pits act as stress raisers. Use coatings, a less corrosive medium or shot peening.
Mean-stress design lines (brief)
Goodman: σa/Se + σm/Su = 1/n     Soderberg: σa/Se + σm/Sy = 1/n     Gerber: σa/Se + (σm/Su)² = 1

Soderberg is the most conservative. Example: Se = 300 MPa, Su = 700 MPa, σm = 150 MPa. Goodman (n = 1) gives allowable σa = 300(1 − 150/700) = 236 MPa.

8. Creep High Asked: End Sem 2024 (4 marks)

Definition

Creep is time-dependent, permanent deformation of a material under a constant load or stress, normally at elevated temperature. For metals it becomes important above about 0.4 Tm (absolute temperature). Examples: turbine blades, steam-line pipes, boiler tubes, nuclear reactor parts. Polymers, and lead at room temperature, creep even at ambient temperature.

Creep curve: the three stages

ε₀ Primary Secondary(steady state) Tertiary ε̇s = Δε/Δt rupture tr Time t Creep strain ε (a) Typical creep curve (constant σ, T) T₃ > T₂ > T₁(or σ₃ > σ₂ > σ₁) Time t (b) Effect of T and σ
Raising temperature or stress raises the instantaneous strain and the steady-state creep rate, and shortens the rupture life (Callister §8.12–8.13).
Model answer: three stages of creep and their mechanisms (4 marks)

Instantaneous strain ε₀ appears on loading. It is mostly elastic.

1. Primary (transient) creep: the creep rate decreases continuously with time, so the curve is concave downward. Mechanism: strain hardening dominates. Dislocations multiply and tangle, so deformation becomes harder as strain increases. Recovery is slower than hardening.

2. Secondary (steady-state) creep: the creep rate is constant, so the curve is linear. This is the longest stage. Mechanism: a balance between strain hardening and recovery (softening). Dislocations escape obstacles by climb, which is aided by vacancy diffusion, and annihilate. Its slope ε̇s is the key design parameter for long-life parts.

3. Tertiary creep: the creep rate accelerates until rupture. Mechanism: microstructural and metallurgical changes: grain-boundary separation, formation of internal cracks, cavities and voids, necking (which raises the true stress), coarsening of precipitates, and recrystallization. Rupture is usually intergranular.

Draw: the curve with the three stages, ε₀, the slope ε̇s, the rupture point and tr.

Effect of stress and temperature, and the creep-rate equation

Formulas
ε̇s = K₁σn   (constant T)      ε̇s = K₂σn exp(−Qc/RT)

n is the stress exponent (about 3–8 for dislocation creep; 1 for diffusion creep). Qc is the activation energy for creep, often about equal to that for self-diffusion. R = 8.314 J/mol·K.

Worked numerical 9: creep rate

(a) At constant temperature, the steady-state creep rate is 2.5 × 10⁻³ h⁻¹ at 200 MPa, and n = 5. Find the rate at 250 MPa.

ε̇₂ = ε̇₁(σ₂/σ₁)n = 2.5 × 10⁻³ × (1.25)⁵ = 2.5 × 10⁻³ × 3.052 = 7.63 × 10⁻³ h⁻¹.

(b) Qc = 270 kJ/mol. By what factor does ε̇s rise from 800 K to 850 K at the same stress?

ε̇₂/ε̇₁ = exp[(Qc/R)(1/T₁ − 1/T₂)] = exp[(270000/8.314)(1/800 − 1/850)] = exp(32475 × 7.353 × 10⁻⁵) = exp(2.388) = ≈ 10.9. A 50 K rise makes creep about 11 times faster.

Mechanisms of creep

MechanismWhat happensDominant when
Dislocation glideDislocations move on slip planes, overcoming obstacles with thermal helpHigh stress
Dislocation climb (power-law creep)Edge dislocations climb out of their slip plane by absorbing or emitting vacancies, bypass obstacles and then glide again. Rate is controlled by diffusion. n ≈ 3–8Intermediate to high stress, T > 0.4Tm
Nabarro–Herring creepVacancies diffuse through the lattice (grain interior) from grain boundaries under tension to those under compression, so grains elongate. ε̇ ∝ σ/d²Low stress, very high T
Coble creepSame idea but diffusion along grain boundaries. ε̇ ∝ σ/d³Low stress, lower T than N–H, fine grains
Grain-boundary slidingGrains slide past each other along the boundaries, which needs accommodation by diffusion or dislocations. Causes wedge cracks and cavities at triple pointsHigh T, fine grains, tertiary stage

A deformation-mechanism map (Ashby) plots σ/G against T/Tm and shows which mechanism dominates in each region.

Data extrapolation: Larson–Miller parameter

Larson–Miller parameter
LM = T (C + log tr)

T in kelvin, tr in hours, C ≈ 20. Short tests at higher temperature are used to predict long-term rupture life at lower temperature for the same stress.

Worked numerical 10 (Callister Ex. 8.2)

Predict the rupture time of an S-590 alloy component at 800 °C (1073 K) and 140 MPa. From the LM plot, LM = 24.0 × 10³ at 140 MPa.

24 000 = 1073(20 + log tr), so log tr = 22.37 − 20 = 2.37 and tr = 233 h (≈ 9.7 days).

Inverse: for 1000 h life at 700 °C, LM = 973(20 + 3) = 22.4 × 10³. Read the allowable stress off the plot at this value.

140 MPa 24×10³ LM = T(20 + log tr) Stress (log)
Larson–Miller plot (sketch).

Effect of material variables and creep-resistant materials

VariableBetter creep resistance with…Reason
Melting pointHigh TmAt a given service T, the homologous temperature T/Tm is lower, so diffusion is slower.
Elastic modulusHigh EStronger bonds
Grain sizeLarge grains, or no grain boundaries at all (single crystal)Fewer boundaries means less grain-boundary sliding and Coble creep. This is the opposite of room-temperature strengthening.
Grain orientationDirectional solidification: grains elongated along the stress axisNo transverse boundaries normal to the stress
Solid-solution alloyingYesSolute atoms impede dislocation motion and slow diffusion.
Precipitates and dispersionsFine, stable particles (e.g. γ′ Ni₃(Al,Ti) in superalloys; ThO₂ in TD-nickel)They pin dislocations and grain boundaries and must not coarsen at service T.

9. Design considerations: summary Medium

Failure modeDesign parameterDesign measures
Brittle fractureKIc, largest flaw aUse KIc design. Use NDT to find flaws. Choose materials whose DBTT is below service temperature. Avoid notches.
FatigueSe or fatigue strength at N cyclesUse fillets and a smooth finish. Shot peen or case harden. Avoid corrosive media. Check mean stress with Goodman or Soderberg.
Creepε̇s, tr (LM parameter)Use high-Tm, coarse-grained or single-crystal precipitation-hardened alloys, and limit the service temperature.

Likely exam questions

  1. Explain Griffith's theory of brittle fracture and derive the expression for the critical stress to propagate a crack. (6)
  2. A material has KIc = 80 MPa√m, critical crack length 0.05 mm and E = 120 GPa. Calculate its surface energy. (2)
  3. Discuss the three stages of the creep curve with a diagram, and explain the mechanism in each stage. (4)
  4. Differentiate between ductile and brittle fracture. Explain cup-and-cone fracture with sketches. (4)
  5. Define fracture toughness. What is plane-strain fracture toughness? A plate with KIc = 50 MPa√m, Y = 1.1 carries 250 MPa: find the critical crack length. (5+3)
  6. What is the ductile-to-brittle transition? Why do BCC metals show it and FCC metals do not? Explain the Charpy test. (4)
  7. Draw S–N curves for steel and aluminium. Define endurance limit and fatigue strength. Explain the factors that improve fatigue life. (6)
  8. Define σm, σa, σr and R. For σmax = 400 MPa and σmin = −100 MPa, find them. (2–3)
  9. Explain the creep mechanisms: dislocation climb, Nabarro–Herring, Coble, grain-boundary sliding. How do material variables affect creep resistance? (4–6)
  10. What is the Larson–Miller parameter? Find the rupture life at 1073 K if LM = 24 × 10³. (3)
  11. Explain the upper and lower yield points and the 0.2 % offset method. Relate E, G and ν. (4)
Model answer: why BCC metals show a DBTT (4 marks)

In BCC metals there is no truly close-packed plane, so the Peierls (lattice friction) stress for dislocation motion is high and strongly temperature-dependent. Dislocation glide needs thermal activation. As temperature falls, the yield stress rises steeply, while the cleavage fracture stress changes little. Below the temperature where the two curves cross (the DBTT), the material cleaves before it can yield: low impact energy, flat granular fracture. FCC metals have 12 close-packed {111}⟨110⟩ slip systems and a low Peierls stress that hardly changes with temperature. Yielding always occurs before cleavage, so they remain ductile down to cryogenic temperatures. That is why austenitic stainless steel, Al and Cu are used for LNG tanks. Sketch the energy–temperature curve for both.

Model answer: improving fatigue life (4 marks)
  1. Design: remove stress raisers. Use generous fillet radii, avoid sharp keyways, and drill crack-stopper holes.
  2. Surface finish: polish to remove machining marks, where cracks start.
  3. Compressive residual stress: shot peening, case hardening (carburizing, nitriding) or surface rolling. The compressive layer offsets the tensile part of the cycle.
  4. Mean stress: reduce σm, keeping within the Goodman line.
  5. Environment: prevent corrosion fatigue with coatings, inhibitors or a cathodic method, and minimise thermal-stress cycling.
  6. Material: choose clean (inclusion-free), fine-grained alloys with a high endurance limit.
Unit 5 · ~6 contact hrs

Composite Materials

Most examined: classification by reinforcement (with tree diagram), rule of mixtures (isostrain/isostress) numericals, critical fibre length, applications.

1. What is a composite? High

Definition

A composite is a multiphase material, normally made artificially, in which the constituent phases are chemically dissimilar and separated by a distinct interface. It combines the best properties of its constituents. This is the principle of combined action: better property combinations come from a judicious mix of two or more distinct materials. Most composites have two phases. The matrix is continuous and surrounds the other phase. The dispersed phase (reinforcement) is embedded in it. Examples: wood (cellulose fibres in lignin), bone, concrete, GFRP, CFRP, WC–Co cermets.

The properties of a composite depend on the properties of the constituent phases, their relative amounts, and the geometry of the dispersed phase: particle shape, size, distribution and orientation.

Functions of the matrix

  • Binds the fibres together and transmits and distributes the applied load to them.
  • Protects the fibres from surface damage (abrasion, chemical attack).
  • Separates the fibres, which stops cracks spreading from fibre to fibre. Cracks are blunted by the ductile matrix.
  • Gives transverse strength, shape and the maximum service temperature.

Functions of the reinforcement

  • Carries most of the load: high strength and stiffness.
  • Raises E, strength, creep and fatigue resistance, and toughness (in ceramic-matrix composites).
  • Particles improve wear resistance, hardness and dimensional stability, and lower cost.
  • The fibre–matrix bond must be strong for load transfer. Coupling agents help (see Unit 6).
Classification by matrixExampleTypical use
Polymer-matrix (PMC)GFRP, CFRP, aramid–epoxyBoat hulls, aircraft parts, sports goods
Metal-matrix (MMC)Al–SiC, Al–B, Al–Al₂O₃ fibresEngine pistons, brake rotors, drive shafts
Ceramic-matrix (CMC)SiC–SiC, Al₂O₃–SiC whiskersCutting tools, turbine parts (higher toughness)
Carbon–carbonCarbon fibres in a carbon matrixBrake discs (aircraft, F1), re-entry nose cones

2. Classification based on reinforcement High

Composites Particle-reinforcedFibre-reinforcedStructural Large-particle Dispersion-strengthened Continuous(aligned) Discontinuous(short) Laminates Sandwichpanels AlignedRandom
Classification scheme for composites by reinforcement (Callister Fig. 16.2). Learn this tree: it is the opening diagram for almost every composite question.

2.1 Particle-reinforced composites

The dispersed phase is equiaxed: particle dimensions are about the same in all directions.

Large-particle compositesDispersion-strengthened composites
Particle sizeLarge (> 1 µm)Very small, 0.01–0.1 µm (10–100 nm)
MechanismParticle–matrix interaction is not at the atomic level. Particles restrain the movement of the matrix near them, so the matrix transfers part of the load to the (stiffer) particles. Analysed by continuum mechanics.Interaction at the atomic or molecular level, as in precipitation hardening. Particles hinder dislocation motion, so yield strength and hardness rise.
Volume fractionOften large, 15–90 %Small, typically < 15 %
PurposeImprove stiffness, wear resistance and hardness; lower costStrength retained at high temperature. Particles are inert and do not coarsen or dissolve, unlike precipitates.
ExamplesConcrete (gravel and sand in cement); cermets such as cemented carbide WC or TiC in a Co or Ni binder (cutting tools); carbon black in vulcanised rubber tyres (15–30 vol %, 20–50 nm); polymers with fillersTD nickel (≈ 3 vol % ThO₂ in Ni); SAP (sintered aluminium powder, Al₂O₃ flakes in Al)
Rule of mixtures for particulate composites (bounds)
Upper bound: Ec(u) = EmVm + EpVp      Lower bound: Ec(l) = EmEp / (VmEp + VpEm)

Vm + Vp = 1. The actual modulus lies between the bounds. Density always follows the linear rule: ρc = ρmVm + ρpVp.

Worked numerical 1: particulate bounds

A composite of 50 vol % tungsten particles (E = 407 GPa) in copper (E = 110 GPa). Find the upper and lower bounds on Ec.

Upper: 0.5(110) + 0.5(407) = 258.5 GPa. Lower: (110 × 407)/(0.5 × 407 + 0.5 × 110) = 44 770/258.5 = 173.2 GPa.

Density (ρCu = 8.96, ρW = 19.3 g/cm³): ρc = 0.5(8.96) + 0.5(19.3) = 14.13 g/cm³.

2.2 Fibre-reinforced composites High

These are technologically the most important. The aim is high specific strength (strength/density) and specific modulus (E/density). The dispersed phase has a large length-to-diameter ratio. By diameter the reinforcement is either a whisker (very thin single crystal, nearly flaw-free, extremely strong, expensive), a fibre (polycrystalline or amorphous, small diameter), or a wire (metallic, larger diameter).

Influence of fibre length: critical fibre length lc

The load is transferred from the matrix to the fibre by shear at the fibre–matrix interface. No load is transferred at the fibre ends. A minimum length, lc, is needed for the fibre to be loaded to its full tensile strength σf*.

Critical fibre length
lc = σf* d / (2τc)

d is the fibre diameter. τc is the fibre–matrix bond strength or the matrix shear yield strength, whichever is smaller. Fibres with l ≫ lc (typically l > 15 lc) behave as continuous. Fibres with l < 15 lc are discontinuous (short). If l < lc, there is hardly any reinforcement and the composite behaves like a particulate one.

σf*σf*σf* (a) l = lc: σf* only at centre (b) l > lc: effective (c) l < lc: never reaches σf*
Stress along a fibre loaded to σf* (Callister Fig. 16.7). The stress builds up from zero at each end over a distance lc/2.
Worked numerical 2: critical fibre length

Carbon fibres (d = 10 µm, σf* = 3.5 GPa) are in an epoxy matrix with bond strength τc = 10 MPa. Find lc and the minimum length for "continuous" behaviour.

lc = (3500 × 10⁶ × 10 × 10⁻⁶)/(2 × 10 × 10⁶) = 35 000/(2 × 10⁷) = 1.75 × 10⁻³ m = 1.75 mm. Continuous behaviour needs l > 15 lc ≈ 26 mm.

Inverse: if lc = 1 mm for a 15 µm glass fibre with σf* = 3.45 GPa, then τc = σf*d/(2lc) = (3450 × 15 × 10⁻⁶)/(2 × 10⁻³) = 25.9 MPa.

Influence of fibre orientation and concentration

(a) Continuous, aligned(b) Discontinuous, aligned(c) Discontinuous, random
Fibre arrangements. Aligned fibres give anisotropic properties: very high along the fibres, low across them. Random short fibres give isotropic but lower properties.

2.3 Continuous, aligned fibre composites: rule of mixtures High

Isostrain (longitudinal)Isostress (transverse)
Grey = fibres. Load parallel to the fibres (left) or perpendicular to them (right).

Longitudinal loading: isostrain

The load is shared: Fc = Fm + Ff, so σcAc = σmAm + σfAf. Divide by Ac: σc = σmVm + σfVf. With perfect bonding, εc = εm = εf. Dividing by ε gives the upper bound:

Ecl = EmVm + EfVf

Transverse loading: isostress

σc = σm = σf and εc = εmVm + εfVf. This gives the lower bound:

1/Ect = Vm/Em + Vf/Ef

All fibre-composite formulas (memorise)
Ecl = EmVm + EfVf     Ect = EmEf/(VmEf + VfEm)
Ff/Fm = EfVf/(EmVm)     (load ratio, isostrain)
Longitudinal strength: σ*cl = σ′m(1 − Vf) + σf*Vf
Discontinuous aligned, l > lc: σ*cd = σf*Vf(1 − lc/2l) + σ′m(1 − Vf)
Discontinuous aligned, l < lc: σ*cd′ = (lτc/d)Vf + σ′m(1 − Vf)
Random / other orientation: Ecd = K EfVf + EmVm

σ′m is the matrix stress at the strain where the fibres fail. K is the fibre efficiency: 1 for aligned (longitudinal), 0 for aligned (transverse), 3/8 for random in-plane (2-D), 1/5 for random 3-D.

Stress–strain behaviour (longitudinal). Stage I: both fibre and matrix are elastic, and the slope is Ecl. Stage II: the matrix yields, the curve is nearly linear but flatter, and the fibres carry almost all the extra load. Failure begins when the fibres break. The failure is gradual, not catastrophic, because fibres break at different points and the matrix still holds pulled-out fibres.

Worked numerical 3: longitudinal modulus and load sharing (Callister Ex. 16.1)

A continuous, aligned glass-fibre/polyester composite has 40 vol % glass fibres (Ef = 69 GPa) in a polyester matrix (Em = 3.4 GPa). (a) Find Ecl. (b) If the cross-section is 250 mm² and the longitudinal stress is 50 MPa, find the load carried by each phase. (c) Find the strain in each phase.

(a) Ecl = 3.4(0.6) + 69(0.4) = 2.04 + 27.6 = 29.6 GPa ≈ 30 GPa.

(b) Ff/Fm = (69 × 0.4)/(3.4 × 0.6) = 27.6/2.04 = 13.5. Total Fc = 50 × 250 = 12 500 N. Fm = 12 500/14.5 = 862 N and Ff = 11 638 N. The fibres carry 93 % of the load.

(c) Am = 150 mm² and Af = 100 mm², so σm = 862/150 = 5.75 MPa and σf = 11 638/100 = 116.4 MPa. εm = 5.75/3400 = 1.69 × 10⁻³; εf = 116.4/69 000 = 1.69 × 10⁻³. They are equal, which confirms isostrain.

Worked numerical 4: transverse modulus

For the same composite: Ect = (3.4 × 69)/(0.6 × 69 + 0.4 × 3.4) = 234.6/(41.4 + 1.36) = 234.6/42.76 = 5.5 GPa. This is about 1/5 of Ecl, which shows the strong anisotropy.

Worked numerical 5: designing Vf; longitudinal strength

(a) What fibre fraction of carbon (Ef = 230 GPa) in epoxy (Em = 3.4 GPa) gives Ecl = 50 GPa?

50 = 3.4(1 − Vf) + 230Vf, so Vf = (50 − 3.4)/(230 − 3.4) = 46.6/226.6 = 0.206 (20.6 %).

(b) Longitudinal tensile strength with Vf = 0.6, σf* = 4000 MPa and σ′m = 15 MPa: σ*cl = 15(0.4) + 4000(0.6) = 6 + 2400 = 2406 MPa.

(c) Random in-plane short glass fibres, Vf = 0.3: Ecd = (3/8)(69)(0.3) + 3.4(0.7) = 7.76 + 2.38 = 10.1 GPa.

Worked numerical 6: discontinuous aligned strength

Fibres with l = 5 mm, lc = 1 mm, σf* = 3.45 GPa, Vf = 0.3 and σ′m = 20 MPa. Since l > lc:

σ*cd = 3450(0.3)(1 − 1/10) + 20(0.7) = 931.5 + 14 = 945.5 MPa.

A continuous composite would give 1035 + 14 = 1049 MPa. Short fibres reach about 90 % of that.

2.4 Structural composites Medium

3. Characteristics, advantages and limitations Medium

Advantages

  • Very high specific strength and specific stiffness, so they are light.
  • Properties can be tailored by choosing the fibre type, Vf and orientation.
  • Good fatigue and corrosion resistance (PMCs do not rust).
  • Low thermal expansion (CFRP), so they are dimensionally stable.
  • Good damping. Complex shapes can be moulded as single parts, which reduces fasteners.
  • Toughness: crack blunting and fibre pull-out, especially in CMCs.

Limitations

  • Anisotropic: weak in the transverse direction and between layers (delamination).
  • High cost (carbon, aramid) and slow manufacture.
  • PMCs have a low maximum service temperature and absorb moisture.
  • Damage can be hidden (impact) and is hard to inspect and repair.
  • Recycling is difficult (thermosets).
  • Joining is difficult. Compressive strength is low for aramid.

4. Applications of composites in industry High

IndustryCompositeApplications
AerospaceCFRP, aramid–epoxy, honeycomb sandwich, C–C, CMCsBoeing 787 and A350 fuselage and wings (~50 % composite by weight), helicopter rotor blades, control surfaces, rocket motor cases, brake discs, re-entry heat shields
AutomotiveGFRP (SMC), CFRP, Al–SiC MMC, rubber + carbon blackBody panels, leaf springs, drive shafts, bumpers, F1 monocoque chassis, pistons, brake rotors, tyres
SportsCFRP, GFRP, aramidTennis rackets, golf shafts, bicycle frames, fishing rods, skis, hockey sticks, pole-vault poles, helmets
MarineGFRP, sandwich (foam/balsa core)Boat and yacht hulls, decks, masts, minesweeper hulls (non-magnetic)
Construction and civilConcrete, RCC, pre-stressed concrete, GFRP rebar, CFRP wrapsBuildings, bridges, column retrofit, pipes, tanks, window frames
ElectricalGFRP (non-conducting), Cu–W, Ag–WPrinted circuit boards (FR-4: glass–epoxy), insulator rods, switchgear, electrical contacts, wind-turbine blades
Cutting tools and wearCermets (WC–Co, TiC–Ni), Al₂O₃–SiC whiskerCutting tool inserts, drill bits, dies, mining tools
Defence and protectionKevlar (aramid), UHMWPE, ceramic/aramidBullet-proof vests, helmets, vehicle armour
BiomedicalCFRP, hydroxyapatite–polymerProsthetic limbs, bone plates, dental fillings (particulate)

Likely exam questions

  1. Define a composite material. Classify composites on the basis of reinforcement, with a neat diagram, giving examples of each. (6)
  2. Differentiate between large-particle and dispersion-strengthened composites. (3–4)
  3. Derive the expressions for the modulus of a continuous, aligned fibre composite under isostrain and isostress conditions. (5)
  4. A composite contains 40 % glass fibres (E = 69 GPa) in polyester (E = 3.4 GPa). Find Ecl, Ect and the fraction of load carried by the fibres. (3–4)
  5. What is critical fibre length? Derive or state lc and explain its significance with stress profiles. (4)
  6. Explain the influence of fibre length, orientation and concentration on composite properties. (4)
  7. Write short notes on laminar composites and sandwich panels. (4)
  8. Discuss the characteristics and applications of composite materials in industry. (4)
  9. What are the functions of the matrix and the reinforcement in a composite? (3)
Model answer: classification of composites based on reinforcement (6 marks)

Definition (1 mark): give the definition from §1. Then draw the tree diagram (2 marks) and explain each class briefly (3 marks):

  1. Particle-reinforced: the dispersed phase is equiaxed.
    • Large-particle: particles over 1 µm restrain the matrix and share the load. Examples: concrete, WC–Co cermet, carbon black in tyres.
    • Dispersion-strengthened: 10–100 nm oxide particles block dislocations, and the strength is retained at high temperature. Examples: TD-Ni (ThO₂), SAP (Al₂O₃ in Al).
  2. Fibre-reinforced: the dispersed phase has a high aspect ratio, and the fibres carry most of the load. These give the best specific strength and stiffness.
    • Continuous aligned: l > 15 lc. Highly anisotropic. Examples: CFRP, GFRP filament-wound tanks.
    • Discontinuous: short fibres, either aligned or randomly oriented (isotropic). Example: chopped-strand GFRP, SMC panels.
  3. Structural: properties depend on the geometric design of the elements as well as the materials.
    • Laminates: plies stacked at different angles. Examples: plywood, CFRP skins.
    • Sandwich panels: stiff faces with a light core (honeycomb or foam). Example: aircraft floors.
Model answer: large-particle vs dispersion-strengthened (3 marks)

Size: > 1 µm versus 0.01–0.1 µm. Mechanism: mechanical restraint of the matrix and load sharing (continuum level) versus blocking of dislocation motion (atomic level). Volume fraction: high (up to 90 %) versus low (< 15 %). Aim: stiffness, wear and cost versus high-temperature strength. Examples: concrete and cemented carbide versus TD-Ni and SAP. Dispersoids, unlike precipitates, do not dissolve or coarsen at high temperature, so the strengthening lasts.

Unit 6 · ~7 contact hrs

Powder Metallurgy & Fibre-Reinforced Composites

Most examined: powder production methods, P/M process steps, cemented carbide manufacture, sintering, self-lubricating bearings, fibres (glass, carbon, Kevlar 49) and matrices, coupling agents.

Part A · Powder Metallurgy (P/M)

Definition

Powder metallurgy is the process of producing metal (or ceramic–metal) parts by compacting fine powders in a die into the required shape, and then sintering them: heating below the melting point of the main constituent in a controlled atmosphere, so that the particles bond by solid-state diffusion. The principle: the powder particles bond and densify by atomic diffusion, driven by the reduction in surface energy, without melting the bulk. It is the method of choice for refractory metals (W, Mo), for materials that do not mix in the liquid state (W–Cu, Cu–graphite), for controlled porosity, and for net-shape mass production.

1. P/M process: flow chart High

1. Powderproduction 2. Characterisationsize, shape, flow 3. Blending+ lubricant, alloying 4. Compactiongreen compact 5. Sintering0.7–0.9 Tm, H₂ gas 6. Secondary opssizing, infiltration 7. Finishingheat / surface treat 8. Inspectionfinished part
Sequence of operations in powder metallurgy. Compaction and sintering (accent) are the two essential steps.

2. Powder production methods High Asked: End Sem 2024

(a) Atomization: the most widely used

A stream of molten metal is broken into fine droplets by high-pressure jets of gas (N₂, Ar, air) or water, or by a spinning disc or electrode (centrifugal atomization). The droplets solidify in flight into powder.

  • Gas atomization gives spherical particles. Water atomization gives irregular particles, which are cheaper and have better green strength.
  • Size range 10–1000 µm. Used for most alloys: steels, stainless steel, Al, Cu, bronze, superalloys.
  • Pre-alloyed powders are possible.
meltgas/waterjetsdropletspowder
Gas or water atomization.

(b) Reduction of oxides (chemical)

Metal oxides are reduced in the solid state by H₂ or CO gas, or by carbon, at temperatures below the melting point. The result is a spongy, porous, irregular powder with good compressibility and green strength. Examples: W, Mo (WO₃ + 3H₂ → W + 3H₂O), Fe sponge powder (Höganäs process), Cu, Ni, Co.

(c) Electrolytic deposition

The metal is deposited at the cathode of an electrolytic cell under conditions (high current density, low metal-ion concentration) that give a loose, spongy or powdery deposit. The deposit is washed, dried, milled and annealed. The powder is of very high purity and dendritic, with excellent compressibility. Examples: Cu (most common), Fe, Ag, Ni, Ta.

(d) Mechanical methods: comminution and mechanical alloying

(e) Carbonyl process (thermal decomposition)

Fe or Ni reacts with CO under pressure to form volatile carbonyls, Fe(CO)₅ or Ni(CO)₄. These are distilled and then decomposed by heating to give very fine (1–10 µm), spherical, high-purity powder. Used for magnetic cores and electronic parts.

(f) Others

Chemical precipitation from solution (Ag, Cu), granulation (pouring molten metal into water), and the hydride–dehydride process (Ti, Zr).

MethodParticle shapePurityTypical metals
Gas atomizationSphericalHighSuperalloys, stainless steel, Al, Ti
Water atomizationIrregularModerate (oxide skin)Steels, Cu, Fe
ReductionSpongy, porousModerate to highW, Mo, Fe, Cu
ElectrolyticDendriticVery highCu, Fe, Ag
Mechanical (milling)Flaky, angularContamination possibleBrittle carbides, oxides
CarbonylFine sphericalVery highFe, Ni

3. Characterisation and blending Medium

4. Compaction High

Powder is pressed in a die at pressures of 70–800 MPa (higher for steel) to form a green compact. The compact has the required shape and enough strength to be handled (green density about 70–90 % of theoretical). Particles first rearrange, then deform plastically at the contacts, and finally interlock and cold-weld.

5. Sintering: mechanism and stages High

Definition

Sintering is heating the green compact to about 0.7–0.9 Tm (absolute) of the main constituent, for a period of time (roughly 10 minutes to several hours), in a protective atmosphere: H₂, dissociated ammonia, endothermic gas, N₂-based gas, or vacuum. The particles bond metallurgically by atomic diffusion, so strength and density rise and porosity falls. Typical temperatures: Fe and steel 1100–1300 °C, Cu 750–1000 °C, bronze 760–870 °C, WC–Co 1400–1500 °C.

(a) Point contactafter pressing (b) Initial stage:neck formation and growth (c) Final stage: grains withisolated spherical pores
Neck growth during sintering. The driving force is the reduction in total surface energy.
  1. Initial stage (bonding, neck formation): atoms diffuse to the contact points and necks form and grow between particles. Densification is small at this stage, but strength rises sharply.
  2. Intermediate stage: necks grow larger and the pores form an interconnected, cylindrical network along the grain edges. This is where most of the densification and shrinkage occurs, as particle centres approach one another. Grains begin to grow.
  3. Final stage: the pores become isolated, spherical and closed (density above ~92 %). They shrink slowly and some are trapped inside grains. Grain growth continues.

Diffusion paths: surface diffusion and evaporation–condensation make the neck grow without shrinkage. Grain-boundary diffusion and volume (lattice) diffusion transport material from the contact zone to the neck, which causes shrinkage and densification.

Liquid-phase sintering: a minor constituent with a lower melting point melts (e.g. Co in WC–Co, Cu in Fe–Cu), wets the solid particles and pulls them together by capillary force. This speeds up densification to near full density. Activated sintering uses small additions (e.g. Ni in W) to accelerate diffusion.

6. Secondary operations and surface treatment Medium

OperationPurpose
SizingRe-pressing a sintered part in a die to improve dimensional accuracy.
Coining and repressingRe-pressing to raise density and strength, and to imprint surface detail. May be followed by re-sintering (double press, double sinter).
InfiltrationThe pores of a sintered skeleton are filled with a molten metal of lower melting point by capillary action, e.g. Cu into an Fe or steel skeleton (raises strength, density, toughness, and seals pores) or Cu or Ag into W (electrical contacts).
ImpregnationThe interconnected pores are filled with oil, grease, wax or polymer resin, by vacuum impregnation. Self-lubricating bearings: porous bronze (Cu–10Sn) or Fe bearings with 20–30 % porosity are impregnated with oil. In service, heat and pressure draw the oil to the surface. They need no external lubrication (fans, appliances, automobiles). Resin impregnation seals parts for pressure-tightness and plating.
Heat treatmentQuench-and-temper and carbonitriding of P/M steels. Steam treatment (≈ 550 °C) forms a Fe₃O₄ (magnetite) layer that seals surface pores and improves wear and corrosion resistance.
Surface treatmentPlating (after sealing), shot peening, case hardening (carburizing, nitriding), and coatings (PVD/CVD for carbides) give wear, corrosion and fatigue resistance.
Machining, joiningCross holes, threads and grooves that cannot be pressed. Welding and brazing.

7. Cemented carbide (WC–Co) tools: production steps High Asked: End Sem 2024

WO₃ → W(H₂) W + C →WC Ball-millWC+Co+wax Dry,granulate Press /presinter LP sinter~1400 °C Diamondgrind CVD/PVDcoat
Production of cemented carbide (WC–Co) cutting-tool inserts.
  1. Tungsten powder: WO₃ or ammonium paratungstate is reduced in hydrogen at 600–900 °C to give fine W powder.
  2. Carburization: W powder is mixed with carbon black and heated to 1400–1600 °C in H₂, giving WC powder (1–10 µm). TiC, TaC or NbC may be added for grades that cut steel (they resist cratering).
  3. Mixing and ball milling: WC is milled with 3–25 % cobalt powder (the binder) in an organic liquid (alcohol, acetone or hexane) for many hours. This coats the WC with Co and refines it. Paraffin wax (1–2 %) is added as a pressing lubricant and temporary binder.
  4. Drying and granulation: spray drying gives free-flowing granules.
  5. Compaction: die pressing (≈ 100–200 MPa), extrusion (rods for drills), or CIP produces an oversized green shape that allows for ~17–22 % linear shrinkage.
  6. Dewaxing and presintering at 800–1150 °C in H₂ or vacuum removes the wax. The part reaches a chalk-like strength and can be machined or shaped at this stage.
  7. Final (liquid-phase) sintering at 1350–1500 °C in vacuum or H₂. Co (with dissolved WC; the eutectic is ~1320 °C) melts, wets the WC grains, draws them together by capillarity, and fills the pores, giving near-full density. Sinter-HIP removes any residual porosity.
  8. Finishing: diamond grinding to size and edge honing.
  9. Coating: CVD or PVD layers of TiN, TiC, TiCN or Al₂O₃ for wear resistance.

Properties: hardness about 90 HRA (1300–1800 HV), retained up to ~1000 °C. More Co gives a tougher but softer tool. Uses: cutting inserts, drills, dies, wire-drawing dies, rock and mining bits.

8. Applications, advantages and limitations of P/M High

ApplicationWhy P/M
Cemented carbide tools (WC–Co, TiC–Ni)WC cannot be melted and cast. A Co binder is needed.
Self-lubricating porous bearings (bronze, Fe)Controlled interconnected porosity holds oil.
Filters (bronze, stainless steel)Controlled pore size and permeability.
Refractory metals: W lamp filaments, Mo heaters, Ta capacitorsMelting points too high for casting (W 3410 °C).
Automotive gears, sprockets, cams, connecting rods, synchroniser hubsNet shape, mass production, little or no machining, low cost.
Magnets (Alnico, Nd–Fe–B, ferrites); soft-magnetic coresFine aligned grains; complex shapes.
Electrical contacts: W–Cu, Ag–W, Ag–CdO; brushes (Cu–graphite)Combine materials that do not alloy in the liquid state.
Friction materials (clutch and brake linings: Cu or Fe + graphite + SiO₂)Mixtures of metals and non-metals.
Aerospace: superalloy discs (HIP), Ti parts; ODS alloysFine, uniform microstructure; dispersion strengthening.

Advantages

  • Net or near-net shape: little or no machining, and close to 97 % material use (minimal scrap).
  • Can make parts from high-melting-point metals (W, Mo) and carbides.
  • Can combine immiscible materials (W–Cu, metal–ceramic, metal–graphite).
  • Controlled porosity: self-lubricating bearings and filters.
  • Fine, uniform grain structure with no segregation (unlike casting).
  • Good surface finish and tolerances. High production rates and automation.
  • Skilled labour is not required. Energy-efficient.

Limitations

  • High cost of powders and dies, so it pays only for large production volumes (> ~10 000 parts).
  • Size and shape limits: press capacity, and undercuts and cross holes cannot be pressed.
  • Residual porosity gives lower strength, ductility and toughness than wrought parts (unless HIP is used).
  • Density variations in tall parts.
  • Some powders (Al, Mg, Ti, Zr) are fire and explosion hazards.
  • Powders oxidise and must be stored carefully.

Part B · Fibre-Reinforced Composites (FRC)

9. General characteristics and applications High

10. Introduction to fibres High

PropertyE-glassS-glassCarbon (PAN, standard to high modulus)Aramid (Kevlar 49)
Specific gravity2.582.491.78–2.151.44
Tensile strength (GPa)3.45≈ 4.61.5–4.83.6–4.1
Elastic modulus (GPa)72.5≈ 86228–724131
Specific modulus (GPa)28.1≈ 34106–40791
Failure strain (%)≈ 4.8≈ 5.40.4–1.8≈ 2.8
CostLowestModerateHighHigh
Key strengthCheap, insulating, chemically resistantHighest-strength glassHighest stiffness, fatigue resistance, low CTE, conductiveLowest density, toughness and impact resistance
WeaknessLow E, abradesCostBrittle, low impact resistance, galvanic corrosion with AlPoor compressive strength, UV and moisture sensitive, hard to cut

Callister Table 16.4; S-glass and failure-strain values are typical handbook figures.

Glass fibres

Carbon fibres

Aramid (Kevlar 49) fibres

11. Matrix types High

MatrixExamplesProperties and roleTypical composites and uses
Polymer (PMC)
most widely used
Thermosets: polyester (cheapest), vinyl ester, epoxy (better properties, moisture resistance), phenolics, polyimides (up to ~230 °C), bismaleimides. Thermoplastics: PEEK, PPS, PEI, nylon, PPLight, easy to process at low temperature, corrosion resistant and cheap. Limited service temperature (polyester/epoxy < ~150–200 °C). Low E. Thermoplastics are tougher and recyclable.GFRP, CFRP, aramid–epoxy: aircraft, boats, sports, auto, pipes
Metal (MMC)Al, Mg, Ti, Cu alloys, superalloysHigher operating temperature, non-flammable, good transverse strength, toughness, electrical and thermal conductivity, resistant to organic fluids. Expensive. Reinforcement–matrix reactions at high temperature are a concern.Al–SiC (pistons, brake rotors, drive shafts), Al–B fibre (space shuttle struts), Al–C (antennas), Cu–C, superalloy–W
Ceramic (CMC)SiC, Si₃N₄, Al₂O₃, ZrO₂, glass-ceramicsVery high temperature and oxidation resistance. Reinforcement (SiC fibres or whiskers) mainly raises fracture toughness, from ~3–5 to 6–20 MPa√m, by crack deflection, fibre bridging and fibre pull-out. Transformation toughening in ZrO₂.Al₂O₃–SiC whisker cutting tools, SiC–SiC turbine and exhaust parts, heat engines
Carbon (C–C)Carbon (from pyrolysed resin)Retains strength above 2000 °C, high thermal-shock resistance. Expensive. Oxidises at high temperature unless coated.Aircraft and F1 brakes, rocket nozzles, re-entry nose cones, hot-pressing dies

12. Coupling agents and fillers Medium

Coupling agents

A coupling agent is a chemical applied to the fibre surface (as part of the sizing) that forms a chemical bridge between the inorganic reinforcement and the organic polymer matrix, and so improves interfacial adhesion. The most common are organosilanes, general formula R–Si(OR′)₃. The –Si(OR′)₃ end hydrolyses to silanol (–Si–OH) groups, which condense with –OH groups on the glass surface (Si–O–Si bonds). The organofunctional group R (vinyl, amino, epoxy, methacrylate) reacts or entangles with the resin. Others: titanates, zirconates, maleic-anhydride-grafted polymers (for natural fibres in PP).

Fillers

Fillers are inexpensive, mostly inert, particulate materials added to the matrix resin, typically 10–50 %. Examples: calcium carbonate, talc, kaolin clay, silica, mica, glass microspheres, wood flour, carbon black and alumina trihydrate.

Likely exam questions

  1. Write any three methods of powder production. Describe the steps in the production of cemented carbide tools. (5) · End Sem 2024
  2. Discuss the reinforcement materials commonly used in polymer-matrix composites and how their properties contribute to overall performance. (6) · End Sem 2024
  3. Explain the powder metallurgy process with a flow chart. State its advantages, limitations and applications. (6)
  4. What is sintering? Explain the mechanism and stages of sintering. What is liquid-phase sintering? (4)
  5. Explain compaction, with cold and hot isostatic pressing. (3–4)
  6. How are self-lubricating bearings made by P/M? Explain infiltration and impregnation. (3)
  7. Compare glass, carbon and Kevlar 49 fibres. (4)
  8. Discuss polymer-, metal- and ceramic-matrix composites with examples. (4–6)
  9. What are coupling agents and fillers? Explain the role of silane coupling agents. (3)
Model answer: three powder production methods + cemented carbide (5 marks: 3 + 2 or 2.5 + 2.5)

1. Atomization: molten metal is poured as a thin stream and disintegrated by high-pressure gas or water jets into droplets that solidify as powder. Gas gives spherical particles, water gives irregular ones. Used for steels, Al, Cu and superalloys. It is the most common method.

2. Reduction: metal oxides are reduced by H₂, CO or carbon below the melting point, e.g. WO₃ + 3H₂ → W + 3H₂O. The powder is spongy and porous with good compressibility. Used for W, Mo, Fe and Cu.

3. Electrolytic deposition: the metal is deposited as a loose, powdery layer on the cathode under high current density, then washed, dried and milled. The powder is very pure and dendritic. Used for Cu and Fe.

(Alternatives: mechanical milling or alloying; the carbonyl process for fine, pure Fe and Ni.)

Cemented carbide tool production:

  1. Make WC by carburizing W powder with carbon at ~1500 °C.
  2. Ball-mill WC with 3–25 % Co binder in alcohol, adding paraffin wax.
  3. Dry and granulate.
  4. Press to an oversized green shape.
  5. Dewax and presinter at ~1000 °C, then shape it while it is chalk-like.
  6. Liquid-phase sinter at 1350–1500 °C in vacuum or H₂. Co melts, wets the WC and densifies the part (~20 % linear shrinkage).
  7. Diamond-grind and hone.
  8. CVD/PVD coat with TiN or Al₂O₃.

Draw the flow chart.

Model answer: reinforcements in polymer-matrix composites and their contribution (6 marks)

Introduction: in a PMC the polymer (epoxy, polyester, vinyl ester, PEEK) is light and tough but weak (E ≈ 3 GPa). The reinforcement carries most of the load. The composite properties follow the rule of mixtures, Ec = EmVm + EfVf, so the fibre's E, σ and ρ dominate.

  1. Glass fibres (E- and S-glass; GFRP): E ≈ 72 GPa, σ ≈ 3.45 GPa, ρ = 2.58. They give high strength at low cost, electrical insulation, chemical resistance and good impact behaviour (high strain to failure). Their modest stiffness limits use in stiffness-critical parts. Uses: boat hulls, pipes, car panels, PCBs.
  2. Carbon fibres (CFRP): E = 230–720 GPa, σ up to 4.8 GPa, ρ ≈ 1.8. They give the highest specific stiffness and strength, excellent fatigue resistance, near-zero CTE (dimensional stability) and conductivity. They are brittle and expensive. Uses: aircraft structures, F1, sports goods.
  3. Aramid (Kevlar 49): E = 131 GPa, σ ≈ 3.6–4.1 GPa, ρ = 1.44, the lowest density. It gives the highest specific tensile strength and outstanding toughness, impact and ballistic resistance and damage tolerance. Its compressive strength is poor. Uses: armour, pressure vessels, hybrid laminates.
  4. Others:
    • UHMWPE (Spectra): very light, ballistic.
    • Boron: high E, stiff aerospace skins.
    • Natural fibres (jute, flax, hemp, sisal): cheap, low-density, renewable; used for auto interiors.
    • Particulate fillers (CaCO₃, talc, silica, glass microspheres, carbon black): raise stiffness and dimensional stability and cut cost.

How they contribute to overall performance:

Add a small fibre comparison table (E, σ, ρ). That alone is worth 1–2 marks.

Previous year paper · fully solved

End Term Exam, November 2024 (ME201n)

B.Tech (ME), 3rd semester · 3 hours · Max. marks 40 · answer any five, all questions carry equal marks

Answers are sized to their marks. Where a long figure is needed, the full drawing is in the unit named in brackets. Copy that figure into your answer.

Q1 (a) Draw the iron–carbon diagram, mark all phases and explain the reactions. 6 marks

Model answer

Diagram: draw the Fe–Fe3C diagram (Unit 3): temperature on the y-axis (up to 1600 °C), wt% C on the x-axis from 0 to 6.70. Mark these points: 1538 °C (Fe melting), 1493 °C peritectic, 1394 °C (δ→γ), 1147 °C eutectic, 912 °C (γ→α), 727 °C eutectoid; compositions 0.022, 0.76, 2.14, 4.30, 6.70 % C.

Phases:

Invariant reactions (F = 0 at constant pressure, three phases in equilibrium):

ReactionTemp.Equation
Peritectic1493 °Cδ (0.09 % C) + L (0.53 % C) → γ (0.17 % C)
Eutectic1147 °CL (4.30 % C) → γ (2.14 % C) + Fe3C (6.70 % C) = ledeburite
Eutectoid727 °Cγ (0.76 % C) → α (0.022 % C) + Fe3C (6.70 % C) = pearlite

Classification: steels below 2.14 % C (hypoeutectoid < 0.76; eutectoid = 0.76; hypereutectoid 0.76–2.14); cast irons 2.14–6.70 % C. Critical lines: A1 (727 °C), A3 (γ/α+γ boundary), Acm (γ/γ+Fe3C boundary).

Q1 (b) Derive the equation for Gibbs’ phase rule. 2 marks

Model answer

Consider a system of C components distributed among P phases in equilibrium.

F = C − P + 2
At constant pressure (metallurgical systems, 1 atm): F = C − P + 1

Example: at the Fe–C eutectoid point, C = 2 and P = 3, so F = 2 − 3 + 1 = 0 (invariant: fixed T and compositions).

Q2 (a) Explain the Griffith theory of brittle fracture and deduce the critical stress for crack propagation. 6 marks

Model answer

Idea: the measured fracture strength of brittle materials is 10–1000 times lower than the theoretical cohesive strength (≈ E/10). Griffith (1920) explained this by assuming every brittle solid contains tiny cracks. Stress concentrates at their tips, so a crack spreads when the elastic strain energy released by its growth is at least the surface energy of the new crack faces.

Setup: an infinite plate of unit thickness under uniform tensile stress σ, containing a through elliptical crack of length 2a perpendicular to σ (draw the plate, the crack 2a and arrows for σ; see Unit 4).

  1. Elastic strain energy released by the crack (plane stress): UE = − πa²σ²/E.
  2. Surface energy of the two new crack faces, each of length 2a: US = 2 × (2a × γs) = 4aγs.
  3. Total energy change: U = 4aγs − πa²σ²/E. U first rises with a, then falls (sketch US, UE and U against a; the maximum is at a*).
  4. Condition for unstable growth: dU/da = 0, so 4γs − 2πaσ²/E = 0.
σc = √( 2Eγs / πa ) (plane stress)
σc = √( 2Eγs / π(1 − ν²)a ) (plane strain)

Conclusions: (i) fracture stress ∝ 1/√a, so bigger cracks fracture at lower stress; (ii) a material with higher E and γs is tougher. Orowan’s modification for metals adds the plastic work γp: σc = √(2E(γs + γp)/πa), where γp ≫ γs. In fracture-mechanics form, σc√(πa) = Kc = √(2Eγ).

Q2 (b) KIc = 80 MPa√m, critical crack length 0.05 mm, E = 120 GPa. Find the surface energy γ. 2 marks

Solution

Griffith: σc = √(2Eγ/πa) and fracture toughness Kc = σc√(πa). Squaring and combining gives Kc² = 2Eγ.

γ = Kc² / 2E = (80 × 10⁶)² / (2 × 120 × 10⁹) = 6.4 × 10¹⁵ / 2.4 × 10¹¹

γ ≈ 2.67 × 10⁴ J/m² (26.7 kJ/m²).

Check via the crack length: σc = K/√(πa) = 80/√(π × 5 × 10⁻⁵) = 6383 MPa, and γ = πaσc²/2E = π(5 × 10⁻⁵)(6.383 × 10⁹)²/(2.4 × 10¹¹) = 2.67 × 10⁴ J/m², the same. The crack length cancels out. The value is huge compared with a true surface energy (~1 J/m²) because it includes plastic work (Orowan). Mention this in one line.

Q3 (a) Any three methods of powder production; steps in producing cemented carbide tools. 5 marks

Model answer

Powder production (any three):

  1. Atomization: a stream of molten metal is broken into droplets by high-pressure water or gas (N2, Ar) jets; the droplets solidify as powder. Used for steel, Al, Cu and alloys. Gas atomization gives spherical particles; water atomization gives irregular ones.
  2. Reduction of oxides: metal oxides are reduced by H2 or CO below the melting point, giving porous “sponge” powder (Fe, W, Mo, Cu). Example: WO3 + 3H2 → W + 3H2O.
  3. Electrolytic deposition: metal is deposited at the cathode from an electrolyte as a brittle, spongy layer, then washed, dried and milled. Gives very pure dendritic powder (Cu, Fe, Ag).
  4. Others: mechanical comminution (ball or hammer milling of brittle materials), carbonyl decomposition (Ni(CO)4 → Ni + 4CO), chemical precipitation.

Cemented carbide (WC–Co) tools:

  1. Make WC powder: W powder (by H2 reduction of WO3) + carbon black, carburized at about 1400–1600 °C.
  2. Mixing / milling: WC + 3–20 % Co (binder), ball-milled for hours in alcohol or hexane with 1–2 % paraffin wax as a pressing lubricant.
  3. Drying and granulation (spray drying) into free-flowing granules.
  4. Compaction: die pressing or cold isostatic pressing into “green” compacts.
  5. Presintering at about 800–1000 °C in H2: removes wax and gives chalk-like strength, so the blank can be shaped or machined.
  6. Liquid-phase sintering at 1350–1500 °C in vacuum or H2: Co melts and wets the WC grains. Expect 15–20 % linear shrinkage and near-full density. Optional HIP removes residual porosity.
  7. Finishing: grinding with diamond wheels, brazing onto a steel shank or use as indexable inserts, then CVD/PVD coating (TiN, TiC, Al2O3).

Q3 (b) Annealing and normalizing: effects on microstructure. 3 marks

Model answer
Full annealingNormalizing
Heating15–40 °C above A3 (hypoeutectoid) or above A1 (hypereutectoid)55–85 °C above A3 or Acm (fully austenitic)
CoolingSlowly, in the furnaceIn still air
MicrostructureCoarse pearlite + pro-eutectoid ferrite (or cementite); large grainsFine pearlite, finer and more uniform grains, more pearlite; cementite network in hypereutectoid steel broken up
PropertiesSoftest, most ductile, best machinability, internal stresses removedHigher strength and hardness than annealed, good toughness, uniform properties
UseBefore cold working or machining; to soften castingsRefine coarse cast/forged grain; before hardening

Add: process annealing (below A1, 550–650 °C) restores ductility of cold-worked low-C steel by recrystallization; spheroidizing (just below A1, long hold) turns the cementite into spheroids for maximum machinability.

Q4 (a) Three stages of the creep curve, with diagram and mechanisms. 4 marks

Model answer

Creep is time-dependent, permanent deformation under constant load (or stress) at high temperature, T > 0.4 Tm. Draw strain against time (Unit 4): instantaneous elastic strain ε0, then three stages ending at rupture (×).

  1. Primary (transient) creep: the creep rate decreases with time. Strain hardening outweighs recovery: dislocations multiply and tangle, and a sub-structure forms.
  2. Secondary (steady-state) creep: constant, minimum creep rate ε̇s, the longest stage. There is a balance between strain hardening and recovery (dislocation climb, cross-slip, polygonization). Mechanisms: dislocation glide + climb (high σ), diffusion creep (Nabarro–Herring through the lattice, Coble along grain boundaries at low σ), grain-boundary sliding. ε̇s = K σⁿ exp(−Qc/RT) is the design parameter.
  3. Tertiary creep: the creep rate accelerates until rupture. Causes: necking (reduced area), cavities and voids at grain boundaries, intergranular microcracks, and metallurgical changes (precipitate coarsening, recrystallization).

Higher stress or temperature raises ε0 and ε̇s and shortens rupture life.

Q4 (b) TTT diagram for eutectoid steel: label regions and products. 4 marks

Model answer

Draw temperature (y) against log time (x) for 0.76 % C steel (Unit 3):

Hardness increases from coarse pearlite to fine pearlite to bainite to martensite. Show 2–3 cooling curves (furnace: coarse P; air: fine P; quench: M) for full marks.

Q5 (a) Procedure for Miller indices in cubic and HCP crystals, with examples. 5 marks

Model answer

Cubic planes (hkl):

  1. Choose an origin not on the plane (shift the origin if the plane passes through it).
  2. Find the intercepts on the x, y, z axes in units of a, b, c (a plane parallel to an axis has intercept ∞).
  3. Take reciprocals.
  4. Clear fractions to the smallest integers; enclose in ( ) with no commas; write a negative index with a bar.

Examples: intercepts (1, ∞, ∞) give (100); (1, 1, ∞) give (110); (1, 1, 1) give (111); (½, 1, ∞) give reciprocals (2, 1, 0), so (210); (1, −1, ½) gives (1 1̄ 2). A family is {hkl}.

Cubic directions [uvw]: head coordinates minus tail coordinates, in units of a; reduce to smallest integers; write in [ ]. Example: from (0,0,0) to (1,1,0) is [110]; from (1,0,0) to (0,1,1) gives (−1,1,1), so [1̄11]. A family is ⟨uvw⟩.

HCP: Miller–Bravais indices (hkil), using four axes: a1, a2, a3 at 120° in the basal plane, and c perpendicular to it.

  1. Find the intercepts on a1, a2, a3, c; take reciprocals; clear fractions.
  2. The third index is redundant: i = −(h + k). Convert from 3-index (hkl) by just inserting i.

Examples: basal plane (0001); prism plane (101̄0); pyramidal plane (101̄1).

HCP directions [UVW] to [uvtw]: u = (2U − V)/3, v = (2V − U)/3, t = −(u + v), w = W. Example: [100] gives u = 2/3, v = −1/3, t = −1/3, w = 0, so [2 1̄ 1̄ 0]. [001] becomes [0001].

Q5 (b) Number of vacancies in copper at 200 °C. Qv = 0.9 eV/atom, k = 8.62 × 10⁻⁵ eV/atom·K, ρ = 8.94 g/cm³, A = 63.55 g/mol. 3 marks

Solution

Step 1, atoms per unit volume: N = NAρ/A = (6.022 × 10²³ × 8.94)/63.55 = 8.47 × 10²² atoms/cm³ = 8.47 × 10²⁸ atoms/m³.

Step 2, temperature: T = 200 + 273 = 473 K; kT = 8.62 × 10⁻⁵ × 473 = 0.04077 eV; Qv/kT = 0.9/0.04077 = 22.07.

Step 3: Nv = N exp(−Qv/kT) = 8.47 × 10²⁸ × exp(−22.07) = 8.47 × 10²⁸ × 2.59 × 10⁻¹⁰

Nv ≈ 2.2 × 10¹⁹ vacancies/m³ (= 2.2 × 10¹³ per cm³). Fraction Nv/N ≈ 2.6 × 10⁻¹⁰.

Q6 (a) Reinforcement materials used in polymer-matrix composites and how their properties contribute to performance. 6 marks

Model answer

In a PMC (epoxy, polyester, vinyl ester, PEEK) the fibres carry most of the load while the matrix binds them, transfers load by shear at the interface and protects the fibres. Main reinforcements:

Fibreρ (g/cm³)σt (GPa)E (GPa)Key features → uses
E-glass (S-glass stronger)2.583.4572.5Cheap, strong, good electrical insulator, corrosion resistant; low stiffness → GFRP boat hulls, pipes, tanks, car bodies, wind blades
Carbon (PAN / pitch)1.78–2.151.5–4.8228–724Highest specific modulus, fatigue resistant, low thermal expansion; costly, brittle → aircraft structures, sports goods, F1
Aramid (Kevlar 49)1.443.6–4.1131Highest specific strength, very tough, impact and cut resistant; poor compressive strength, absorbs moisture → body armour, helmets, ropes, tyres, pressure vessels
OthersNatural fibres (jute, flax: cheap, light, eco-friendly), UHMWPE, boron; particulate fillers (silica, CaCO3, carbon black) for stiffness, cost and wear

How they improve the composite:

Q6 (b) Composition, properties and applications of duralumin and brass. 2 marks

Model answer
DuraluminBrass
CompositionAl + 3.5–4.5 % Cu, 0.4–0.8 % Mg, 0.4–0.7 % Mn, ~0.5 % SiCu + Zn (e.g. 70/30 cartridge brass; 60/40 Muntz metal)
PropertiesAge-hardenable; high strength-to-weight (UTS ~400–450 MPa); good machinability; poor corrosion resistance, so used clad (Alclad)Ductile (α-brass cold-workable), good corrosion resistance, golden colour, easily machined (with Pb), good conductivity
UsesAircraft structures and skins, rivets, truck bodies, automobile partsCartridge cases, radiators, plumbing fittings, condenser tubes, musical instruments, coins
Previous year paper · fully solved

Mid Term Exam, March 2024

B.Tech 2nd sem, PE-104 Engineering Materials and Metallurgy · 1.5 hours · 20 marks. Same syllabus; questions like these appear as part (b)s in the end term.

Q1. Planar density of the (110) plane of FCC in terms of r. 2.5 marks

Solution

The (110) plane in an FCC cell is a rectangle of sides a (cube edge) and a√2 (face diagonal).

Atoms centred on the plane: 4 corners × ¼ + 2 face-centre atoms (mid-points of the long sides) × ½ = 2 atoms.

For FCC, a = 2r√2, so area = a × a√2 = (2r√2)(4r) = 8√2 r².

PD110 = 2 / (8√2 r²) = 1 / (4√2 r²) ≈ 0.177 / r²

OR: Define APF and find it for simple cubic.

Solution

APF = volume of atoms in a unit cell ÷ total unit cell volume (atoms taken as hard spheres).

SC: 8 corners × ⅛ = 1 atom; atoms touch along the edge, so a = 2r.

APF = (1 × 4/3 πr³)/(2r)³ = π/6 = 0.52

Q2. BCC iron, (220) planes: (i) interplanar spacing, (ii) diffraction angle. a = 0.2866 nm, λ = 0.1790 nm, n = 1. 5 marks

Solution

(i) dhkl = a / √(h² + k² + l²) = 0.2866 / √(4 + 4 + 0) = 0.2866 / 2.828 = 0.1013 nm

(ii) Bragg’s law nλ = 2d sin θ, so sin θ = (1 × 0.1790)/(2 × 0.1013) = 0.8833

θ = 62.04°, so diffraction angle 2θ = 124.1°

(220) reflects in BCC because h + k + l = 4 is even (BCC rule). In FCC, h, k, l must be all odd or all even.

OR: Relationship between a and r for SC, BCC and FCC.

Solution
StructureAtoms touch alongGeometryResult
SCCube edgea = r + ra = 2r
BCCBody diagonal (a√3)a√3 = 4ra = 4r/√3
FCCFace diagonal (a√2)a√2 = 4ra = 2√2 r

Draw the cube face (FCC) and the body-diagonal section (BCC) with the touching atoms (Unit 1).

Q3. Differentiate edge and screw dislocations with diagrams. 2.5 marks

Model answer
Edge dislocationScrew dislocation
Extra half-plane of atoms inserted in the crystal; symbol ⊥Atoms arranged in a spiral (helical) ramp around the line; symbol ↻
Burgers vector b ⊥ dislocation lineBurgers vector b ∥ dislocation line
Moves (glides) parallel to b, in the direction of applied shearMoves perpendicular to b (and to the shear stress)
Has a unique slip plane; can climb (by diffusion)No unique slip plane, so can cross-slip; cannot climb
Compressive stress above the slip plane, tensile belowPure shear strain field

Draw both with a Burgers circuit, showing the closure failure b (Unit 1). Real dislocations are usually mixed.

OR: Axial relationships and inter-axial angles of the crystal systems.

Model answer
SystemAxial lengthsInter-axial anglesExample
Cubica = b = cα = β = γ = 90°Fe, Cu, NaCl
Hexagonala = b ≠ cα = β = 90°, γ = 120°Zn, Mg, Ti
Tetragonala = b ≠ cα = β = γ = 90°β-Sn, TiO2
Rhombohedral (trigonal)a = b = cα = β = γ ≠ 90°Calcite, Bi
Orthorhombica ≠ b ≠ cα = β = γ = 90°α-S, Ga
Monoclinica ≠ b ≠ cα = γ = 90° ≠ βGypsum
Triclinica ≠ b ≠ cα ≠ β ≠ γ ≠ 90°K2Cr2O7

7 crystal systems combine with lattice centring to give 14 Bravais lattices.

Q4. What is a single crystal? Discuss the various imperfections in a crystal. 5 marks

Model answer

Single crystal: a solid in which the periodic, repeating atomic arrangement extends unbroken through the whole specimen, with no grain boundaries. Properties are anisotropic. Examples: silicon wafers, quartz oscillators, Ni-superalloy turbine blades (creep resistance). A polycrystal is made of many grains of different orientation separated by grain boundaries.

Imperfections, classified by dimension:

  1. Point (0-D): vacancy (missing atom; Nv = N exp(−Qv/kT)); self-interstitial; substitutional and interstitial impurity atoms (solid solutions, Hume-Rothery rules); in ionic crystals the Frenkel defect (cation vacancy + cation interstitial pair) and Schottky defect (cation + anion vacancy pair).
  2. Line (1-D): dislocations: edge (extra half-plane, b ⊥ line), screw (b ∥ line), mixed. They cause plastic deformation by slip at low stress; their interaction gives work hardening.
  3. Surface / planar (2-D): external surfaces; grain boundaries (high- and low-angle, tilt and twist); twin boundaries (mirror-image lattice); stacking faults (ABCABABC in FCC); phase boundaries.
  4. Volume (3-D): pores, cracks, voids, foreign inclusions, precipitates.

Draw: vacancy/interstitial/substitutional in a 2-D atom grid; edge dislocation; grain boundary and twin boundary (Unit 1).

Q5. Draw the iron–carbon phase diagram and describe the invariant reactions. 5 marks

Same as End Sem 2024, Q1(a) above. Drawing the diagram with the peritectic, eutectic and eutectoid reactions at their correct temperatures and compositions earns most of the marks.

Last hour

Formula sheet & final revision

Everything you need for the 2- and 3-mark numerical parts on two pages. Read it right before entering the hall.

Unit 1: Crystal structure and defects

SCBCCFCCHCP
a in terms of r2r4r/√32√2 ra = 2r, c/a = 1.633
Atoms per cell (n)1246
Coordination number681212
APF0.520.680.740.74
ExamplesPoα-Fe, Cr, W, Moγ-Fe, Al, Cu, Ni, AuZn, Mg, Ti, Co
ρ = nA / (Vc NA), NA = 6.022 × 10²³
dhkl = a / √(h² + k² + l²)
Bragg: nλ = 2d sin θ
LD = atoms centred on line / line length
PD = atoms centred on plane / plane area
HCP: i = −(h + k)
[UVW]→[uvtw]: u = (2U−V)/3, v = (2V−U)/3, t = −(u+v), w = W
Nv = N exp(−Qv/kT), N = NAρ/A
k = 8.62 × 10⁻⁵ eV/K = 1.38 × 10⁻²³ J/K
Schmid: τR = σ cos φ cos λ
Hall–Petch: σy = σ0 + ky d−½
%CW = (A0 − Ad)/A0 × 100
Trecryst ≈ 0.3–0.5 Tm (in K)

Planar densities: FCC (100) = 1/(4r²) = 0.25/r²; FCC (110) = 1/(4√2 r²) = 0.177/r²; FCC (111) = 1/(2√3 r²) = 0.289/r² (densest); BCC (110) = 3/(8√2 r²) = 0.265/r² (densest in BCC). Linear: FCC [110] = 1/(2r); BCC [111] = 1/(2r). Slip systems: FCC {111}⟨110⟩ 12; BCC {110}⟨111⟩ 12 (48 in total); HCP (0001)⟨112̄0⟩ 3. Diffraction rules: BCC: h + k + l even; FCC: h, k, l all odd or all even.

Unit 2: Corrosion

Anode (oxidation): M → Mn+ + ne⁻
Cathode: O2 + 2H2O + 4e⁻ → 4OH⁻ (neutral)
2H⁺ + 2e⁻ → H2 (acid)
Ecell = E°cathode − E°anode
Rust: Fe → Fe²⁺ + 2e⁻; Fe²⁺ + 2OH⁻ → Fe(OH)2
4Fe(OH)2 + O2 + 2H2O → 4Fe(OH)3 (→ Fe2O3·nH2O)
Faraday: w = ItM / nF, F = 96 500 C/mol
CPR = KW / ρAt (K = 87.6 → mm/yr)

The more active (anodic) metal corrodes. Small anode + large cathode = rapid attack. Protection methods: material selection, coatings (paint, galvanizing, tinning), cathodic protection (sacrificial Zn/Mg anode or impressed current), anodizing, inhibitors, good design (avoid crevices and dissimilar-metal contact).

Unit 3: Phase diagrams and heat treatment

Gibbs: F = C − P + 2 (F = C − P + 1 at const. P)
Lever rule: WL = (Cα − C0)/(Cα − CL)
Wα = (C0 − CL)/(Cα − CL)
r* = −2γ/ΔGv, ΔG* = 16πγ³ / 3(ΔGv)²
ΔGv = ΔHf(Tm − T)/Tm
Hypo (C0 < 0.76): WP = (C0 − 0.022)/0.74
Wα′ = (0.76 − C0)/0.74
Hyper (C1 > 0.76): WP = (6.70 − C1)/5.94
WFe3C′ = (C1 − 0.76)/5.94
Total: Wα = (6.70 − C0)/6.68, WFe3C = (C0 − 0.022)/6.68
Key Fe–C numbersValueKey Fe–C numbersValue
Peritectic1493 °C: δ(0.09) + L(0.53) → γ(0.17)Max C in α / γ0.022 % (727 °C) / 2.14 % (1147 °C)
Eutectic1147 °C: L(4.30) → γ(2.14) + Fe3CFe3C6.70 % C
Eutectoid727 °C: γ(0.76) → α(0.022) + Fe3CFe melting / δ→γ / γ→α1538 / 1394 / 912 °C
TTT nose (eutectoid)~540 °C, ~1 sMs (eutectoid)~220 °C

Heat treatment temperatures: full anneal A3 + 15–40 °C (furnace cool); normalize A3/Acm + 55–85 °C (air cool) (Callister values; some Indian texts quote 30–50 / 40–60 °C, both accepted); harden A3 + 30–50 °C (hypo) or A1 + 30–50 °C (hyper), water/oil quench; temper 150–650 °C; process anneal 550–650 °C; spheroidize just below A1. Case hardening: carburizing 870–950 °C; nitriding 500–550 °C (no quench); cyaniding 800–870 °C (NaCN bath). Al–4 % Cu: solution treat ~550 °C, quench, age (natural at RT, or artificial 100–200 °C). Sequence: GP zones → θ″ → θ′ → θ (CuAl2); peak, then overaged.

Unit 4: Fracture, fatigue, creep

σ = F/A0, ε = Δl/l0, E = σ/ε
E = 2G(1 + ν)
σT = σ(1 + ε), εT = ln(1 + ε)
Griffith: σc = √(2Eγs/πa)
σm = 2σ0√(a/ρt), Kt = σm/σ0
KIc = Yσ√(πa); Kc² = 2Eγ (→ γ = K²/2E)
Plane strain if B ≥ 2.5(KIc/σy)²
σm = (σmax + σmin)/2
σa = (σmax − σmin)/2, σr = 2σa
R = σmin/σmax (fully reversed R = −1)
Paris: da/dN = A(ΔK)m
Creep: ε̇s = K1σⁿ; ε̇s = K2σⁿ exp(−Qc/RT)
LMP = T(C + log tr), C ≈ 20, T in K, tr in h
Creep significant above ~0.4 Tm

a = surface crack length or half the internal crack length (internal crack = 2a). Units: MPa√m = MN·m⁻³ᐟ²; γ in J/m². Use the same unit system throughout (Pa and m).

Units 5–6: Composites and powder metallurgy

Isostrain (longitudinal): Ecl = EmVm + EfVf
Isostress (transverse): Ect = EmEf / (VmEf + VfEm)
Ff/Fm = EfVf / EmVm
ρc = ρmVm + ρfVf
Critical length: lc = σf* d / 2τc
σ*cl = σ′m(1 − Vf) + σ*fVf
l > lc: σ*cd = σ*fVf(1 − lc/2l) + σ′m(1 − Vf)
Porosity = 1 − ρ/ρtheoretical

Continuous fibres: l > 15 lc. Fibre efficiency factor K: aligned 1, random in a plane 3/8, random in 3-D 1/5. Fibres: E-glass E ≈ 72 GPa, carbon 230–720 GPa, Kevlar 49 131 GPa (ρ = 1.44, highest specific strength).

Must-draw diagrams checklist

Answer-writing checklist